All-IMC-phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection and preparation method of all-IMC-phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder
Through the use of Sn-Bi-In-Ag-Zn high-entropy low-temperature solder, combined with high-entropy alloy and molten eutectic molten salt protection, the existing solder is solved in chip interconnection with brittle and creep resistance. The best problem is that the solder joints with low melting point and high shear strength can be achieved, and the interconnection needs of high computing power chips are met.
Patent Information
- Application Number
- CN202411113336.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
AI Technical Summary
Existing low-temperature solder has problems of hard and brittleness and poor creep resistance in chip interconnection, which is difficult to meet the needs of high-computing chips for intermediary warping and solder joint miniaturization, and the solder's diffusion barrier capability is insufficient.
Using all IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder, the rapid growth of interface IMC is inhibited through the high-entropy effect and hysteresis diffusion effect of high-entropy alloy, and combined with the protection of KCl and LiCl molten eutectic salts, it is prepared. High entropy alloy solder with low melting point and good wetting properties are produced.
It realizes long-term reliability and high shear strength of solder joints, reduces packaging temperature, inhibits the rapid growth of interface IMC, ensures the continuity and stability of solder joints, and meets the interconnection needs of high computing chips.
Smart Images

Figure CN118951476A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a full IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection and a preparation method thereof, belonging to the technical field of electronic packaging materials. Technical Background
[0002] The rise and rapid development of artificial intelligence has greatly increased the demand for high-computing chips. As Moore's Law approaches its limit, the difficulty and cost of optimizing transistor architecture and improving integration density in the front-end process continue to increase. The chip interconnection technology involved in the back-end process has become the key to solving the demand for high-computing chips. Advanced packaging technologies such as embedded IC, fan-out packaging technology (Fan out), flip chip technology (FC), wafer-level chip size package (WLCSP), three-dimensional wafer-level packaging technology (3DWLCSP), three-dimensional chip packaging (3DIC) technology and 2.5D adapter board technology have developed rapidly.
[0003] The application of advanced packaging technology has increased the density of input / output ports and reduced the size of the package body, which has forced interconnection materials to face a more stringent service environment. New requirements have been put forward for interconnection materials between chips: (1) The warping problem of the interposer and the glass transition of the organic substrate require the solder to have a low melting point; (2) The miniaturization of the solder joints increases the volume proportion of IMC in the solder joints, requiring the solder to have good diffusion barrier capabilities to ensure that the interface IMC is continuous and has a slow growth rate. Existing low-temperature solders such as eutectic SnBi and eutectic SnIn have the problems of hardness and brittleness and poor creep resistance, so there is an urgent need for a new type of solder with good diffusion barrier properties and a low melting point to fill the gap.
[0004] High entropy alloy (HEA) refers to a multi-component alloy with a mixing entropy higher than 1.62R or more than 5 main elements, and the atomic ratio of each component is between 5% and 35%. High entropy alloys have high entropy effect and hysteresis diffusion effect, which can inhibit the formation and growth of IMC from the thermodynamic and kinetic perspectives respectively. High entropy alloys also have a high entropy alloy cocktail effect, and the desired properties can be obtained by selecting suitable metals. Studies have shown that the high entropy of Sn-based solders can significantly reduce the melting point of the solder and achieve the inhibition of the rapid growth of interface IMC, which has considerable practical application value in the field of chip interconnection. Summary of the invention
[0005] Aiming at the high reliability requirement of chip interconnection, the present invention provides a Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection and a preparation method thereof. Thanks to the high entropy effect and hysteresis diffusion effect of high entropy alloy, the interface IMC grows slowly during the reflow process, the rapid growth of the interface brittle IMC is suppressed, and a thin IMC layer can still be maintained after a long reflow, which is beneficial to improving the reliability of the solder joint.
[0006] Aiming at the demand for low-temperature interconnection of advanced packaging chips, the present invention provides a full IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection and a preparation method thereof, which has a low melting point, good wetting properties on a Cu substrate and high shear strength.
[0007] In order to achieve the above objectives, the present invention adopts the following technical solutions:
[0008] The full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection of the present invention has the following components in atomic percentage: 25%-35% tin, 21%-35% bismuth, 25%-35% indium, 5% silver and 5%-10% zinc.
[0009] The preparation method of the full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection described in the present invention is as follows: (1) Weigh high-purity Sn, In, Bi, and Ag particles according to the designed proportion, and cover them with 1.3:1 KCl and LiCl molten eutectic molten salt for protection, and smelt the Sn-In-Bi-Ag quaternary master alloy. And put Sn, In, Bi, and Ag in the order of low-density metal at the bottom and high-density metal at the top to reduce the specific gravity segregation during the smelting process, keep warm at 800°C-900°C for 1h-2h and stir thoroughly, and directly cast in water for cooling. (2) Weigh high-purity Zn particles and Sn-In-Bi-Ag quaternary master alloy according to the designed proportion, and place the Sn-In-Bi-Ag quaternary master alloy on the Zn particles for protection. The molten KCl and LiCl eutectic molten salts are poured onto the surface of the metal raw material, kept at 500°C for 1h-2h and fully stirred, and then directly cast into water and cooled to obtain the Sn-Bi-In-Ag-Zn high entropy alloy solder.
[0010] The all-IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection described in the present invention has all phases of IMC phases, mainly InSn4-γ, InBi phase and AgZn phase, among which InSn4-γ is similar to a solid solution, bismuth atoms are highly dissolved in InSn4-γ, with a solid solubility of 9At.%-11At.%, and has a high mixing entropy.
[0011] The full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection of the present invention has a melting point below 85°C, significantly reduces the packaging temperature, and can effectively reduce the warping problem caused by the reflow process. At the same time, at the reflow temperature of 120°C and 150°C, the wetting and spreading rate on the Cu substrate can reach 62% and 69% respectively.
[0012] The full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection of the present invention has good low-temperature welding performance, can realize reliable copper-copper interconnection at 120°C, and can realize reliable copper-copper interconnection at low temperature. At the same time, it has good thermal stability. After reflowing at 120°C-150°C for 5 minutes, the shear strength of the solder joint is ≥33MPa, and after reflowing for 10min and 20min, it is ≥30MPa.
[0013] The full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection of the present invention has conventional Cu6Sn5 as the interface IMC, which ensures connection reliability. At the same time, thanks to the high entropy effect and slow diffusion effect of the high entropy alloy, the rapid growth of the interface IMC is suppressed, and the interface IMC grows uniformly, ensuring the long-term reliability of the solder joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a SEM image of the full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder used for chip interconnection in Example 1 of the present invention;
[0015] Figure 2 The XRD result of the full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection in Example 1 of the present invention;
[0016] Figure 3 This is a DSC curve of the full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection in Example 1 of the present invention;
[0017] Figure 4 This is a SEM image of a Sn-Bi-In-Ag-Zn / Cu solder joint prepared by reflowing the all-IMC Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection at 120° C. for 20 minutes in Example 1 of the present invention; Specific implementation plan
[0018] Implementation Case 1:
[0019] The components of the full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection in this example are calculated in atomic percentage, and its components are 35% tin, 20% bismuth, 35% indium, 5% silver and 5% zinc.
[0020] Weigh high-purity Sn, In, Bi, and Ag particles according to the designed ratio, and cover them with 1.3:1 KCl and LiCl molten eutectic molten salt for protection, and melt Sn-In-Bi-Ag quaternary master alloy. Add Sn, In, Bi, and Ag in the order of low-density metal at the bottom and high-density metal at the top to reduce specific gravity segregation during the smelting process, keep the temperature at 850℃ for 2h and stir thoroughly, and directly cast it in water to cool.
[0021] High-purity Zn particles and Sn-In-Bi-Ag quaternary master alloy were weighed according to the designed proportion, and the Sn-In-Bi-Ag quaternary master alloy was placed on the Zn particles for protection. The molten KCl and LiCl eutectic salts were poured on the surface of the metal raw material, kept at 500°C for 1h and fully stirred, and directly cast in water for cooling to obtain the Sn-Bi-In-Ag-Zn high entropy alloy solder.
[0022] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection and a preparation method thereof. The materials are all IMC phases, mainly InSn4-γ, InBi phase and AgZn phase, among which InSn4-γ is similar to a solid solution, and bismuth atoms are highly dissolved in InSn4-γ with a solid solubility of 11.3At.%, and have high mixing entropy.
[0023] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection and a preparation method thereof, which has a melting point of 84.75°C and a spreading rate of 65.41% and 71.42% when wetting on a Cu substrate at 120°C and 150°C.
[0024] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection and a preparation method thereof. After reflow at 120°C for 5min, 10min, and 20min, the interface shear strength is ≥36.41MPa, 32.49MPa, and 31.04MPa.
[0025] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection and a preparation method thereof. After reflow at 120°C for 5, 10, and 20 minutes, the interface IMC thickness is ≤2.5μm.
[0026] Implementation Case 2:
[0027] The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder used for packaging in this example has a composition, in terms of atomic percentage, of 30% tin, 20% bismuth, 35% indium, 5% silver and 10% zinc.
[0028] Weigh high-purity Sn, In, Bi, and Ag particles according to the designed ratio, and cover them with 1.3:1 KCl and LiCl molten eutectic molten salt for protection, and melt Sn-In-Bi-Ag quaternary master alloy. Add Sn, In, Bi, and Ag in the order of low-density metal at the bottom and high-density metal at the top to reduce specific gravity segregation during the smelting process, keep the temperature at 850℃ for 2h and stir thoroughly, and directly cast it in water to cool.
[0029] High-purity Zn particles and Sn-In-Bi-Ag quaternary master alloy were weighed according to the designed proportion, and the Sn-In-Bi-Ag quaternary master alloy was placed on the Zn particles for protection. The molten KCl and LiCl eutectic salts were poured on the surface of the metal raw material, kept at 500°C for 1h and fully stirred, and directly cast in water for cooling to obtain the Sn-Bi-In-Ag-Zn high entropy alloy solder.
[0030] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high-entropy low-temperature solder for chip interconnection and a preparation method thereof. The materials are all IMC phases, mainly InSn4-γ, InBi phase and AgZn phase, among which InSn4-γ is similar to a solid solution, and bismuth atoms are highly dissolved in InSn4-γ with a solid solubility of 10.1At.%, and have high mixing entropy.
[0031] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection and its preparation method, which has a melting point of 86.1°C and a spreading rate of up to 63.12% when wetted on a Cu substrate at 120°C and 150°C. and 69.66%.
[0032] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection and a preparation method thereof. After reflow at 120°C for 5min, 10min, and 20min, the interface shear strength is ≥37.76MPa, 33.12MPa, and 35.61MPa.
[0033] This example provides a full IMC phase Sn-Bi-In-Ag-Zn high entropy low-temperature solder for chip interconnection and a preparation method thereof. After reflow at 120°C for 5, 10, and 20 minutes, the interface IMC thickness is ≤2.3μm.
[0034] The above embodiments are only preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be regarded as equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. Bismuth, indium, silver and zinc, the composition in atomic percentage is 25%-35% tin, 10%-26% bismuth, 25%-35% indium, 5% silver and 5%-10% zinc.
2. The all-IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection as claimed in claim 1, characterized in that: The solder contains 25% tin, 5% silver, 5%-10% zinc, ≤26% bismuth and the balance indium.
3. The all-IMC phase Sn-Bi-In-Ag-Zn high entropy low temperature solder for chip interconnection as claimed in claim 1, characterized in that: The solder contains 30% tin, 5% silver, 5%-10% zinc, ≤23% bismuth and the balance indium.
4. The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claim 1, characterized in that: The solder contains 35% tin, 5% silver, 5%-10% zinc, ≤20% bismuth and the balance indium.
5. The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claims 1-4, characterized in that: The phases of the high entropy solder are all IMC phases, namely InSn4-γ phase, InBi phase and AgZn phase. Among them, InSn4-γ phase is similar to a solid solution, and bismuth atoms are highly dissolved in InSn4-γ with a solid solubility of 9At.%-11At.%, and has a high mixing entropy.
6. The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claims 1-5, characterized in that: It has an extremely low melting point and good low-temperature wetting performance, which significantly reduces the packaging temperature and can effectively reduce the warping problem caused by CET mismatch during the reflow process. Its melting point is <90℃, and the spreading rate is ≥63% when wetted on a copper substrate at 120℃-150℃.
7. The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claims 1-6, characterized in that: Reliable copper-copper interconnection can be achieved at low temperature. At the same time, the solder joints have good thermal stability after welding. After reflow at 120℃-150℃ for 5 minutes, the shear strength of the solder joints is ≥33MPa, and after reflow for 10min and 20min, it is ≥30MPa.
8. The Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claims 1-7, characterized in that: The interface IMC grows slowly and can maintain a thin IMC layer after long-term reflow. After reflow at 100℃-120℃ for 5-20min, the interface IMC thickness is ≤2.5μm.
9. The method for preparing the Sn-Bi-In-Ag-Zn full IMC phase high entropy low temperature solder for packaging as claimed in claims 1-8, characterized in that: (1) Weigh high-purity Sn, In, Bi, and Ag particles according to the designed ratio, and cover them with 1.3:1 KCl and LiCl molten eutectic molten salt for protection, and melt the Sn-In-Bi-Ag quaternary master alloy. Add Sn, In, Bi, and Ag in the order of low-density metal at the bottom and high-density metal at the top to reduce the specific gravity segregation during the smelting process, keep it at 800℃-900℃ for 1h-2h and stir it thoroughly, and directly cast it into water to cool. (2) Weigh high-purity Zn particles and Sn-In-Bi-Ag quaternary master alloy according to the designed ratio, and place the Sn-In-Bi-Ag quaternary master alloy on the Zn particles for protection. Pour the molten KCl and LiCl eutectic molten salt on the surface of the metal raw material, keep it at 500℃ for 1h-2h and stir it thoroughly, and directly cast it into water to cool to obtain Sn-Bi-In-Ag-Zn high entropy alloy solder.
Citation Information
Cited By
Multi-component tin-indium system lead-free low-temperature solder and preparation method thereof
CN120901549A
A multi-component tin-indium based lead-free low temperature solder and a method for producing the same