Composite barrier film with flame retardance and preparation method thereof

The composite barrier film, which is made by co-extrusion of flame-retardant PET film and heat-sealing PP film, solves the problem of insufficient flame retardancy and heat-sealing performance of PET film, and achieves high flame retardancy and excellent heat-sealing performance, thereby enhancing the barrier and mechanical properties of the film.

CN118952794APending Publication Date: 2024-11-15JIAXING UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411005857.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing PET films have shortcomings in terms of flame retardancy and heat-sealing performance, especially in that they are easily combustible at high temperatures and have poor heat-sealing properties.

Method used

A composite barrier film is made by direct co-extrusion of a flame-retardant PET film layer and a heat-sealable PP film layer. The flame-retardant PET film layer is enhanced with modified PET resin and nano-alumina-coated red phosphorus flame retardant, while the heat-sealable PP film layer is improved with zinc metaborate to enhance compatibility and stability.

Benefits of technology

It achieves excellent heat-sealing performance while improving flame retardant performance, enhances the barrier and mechanical properties of the composite film, and forms a dense network structure to improve flame retardant effect and oxygen barrier effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962993950000021
    Figure BDA0004962993950000021
  • Figure BDA0004962993950000022
    Figure BDA0004962993950000022
  • Figure BDA0004962993950000121
    Figure BDA0004962993950000121
Patent Text Reader

Abstract

The invention discloses a flame-retardant composite barrier film and a preparation method thereof, the composite barrier film is prepared by direct co-extrusion of a flame-retardant PET film layer and a heat-sealing PP film layer, the excellent heat-sealing performance of the PP film can be maintained, and the flame-retardant effect of the composite film can be further improved. PET resin used by the flame-retardant PET film layer is aminated, and MDI and polyacrylic resin are combined for use, so that a formed network structure is more compact, the barrier property of the composite film is enhanced, and flame retardance is facilitated to a certain extent; the further filling of the coated nano flame retardant and nano zinc oxide improves the mechanical properties of the film and enhances the flame retardant effect, and the increase of the density is beneficial to the barrier effect of oxygen and the like. The PP film layer not only guarantees the heat sealing performance, but also enhances the compatibility of the film due to the addition of zinc metaborate, contributes to the formation of a three-dimensional network structure of the composite film, and is good in structural stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite barrier film preparation, and in particular to a composite barrier film with flame retardancy and a preparation method thereof. Background Art

[0002] PET film is a film made of polyethylene terephthalate and is a commonly used packaging material. It has excellent physical properties such as high strength, high modulus, excellent tear resistance and abrasion resistance. In the packaging film market, flame retardancy is a very important factor. Flame retardancy refers to the property that a material does not burn or is difficult to burn under flame or high temperature conditions. The flame retardant V1 level of PET film means that in the vertical burning test of PET film, the flame spread time does not exceed 10 seconds and there is no dripping phenomenon. This means that PET film has good flame retardant properties and can effectively reduce the occurrence of fire accidents. In addition, PET film also has good weather resistance and chemical corrosion resistance.

[0003] Due to the high combustion temperature of fire, the flame retardant temperature is required to reach 260℃ or even higher, which further upgrades the flame retardancy requirements. In addition, PET packaging films have poor heat sealing performance. Therefore, we use polypropylene with excellent heat sealing performance for compounding, and compound PET film with PP film under the premise of meeting the flame retardancy requirements and not affecting other properties.

[0004] In the present invention, we disclose a composite barrier film with flame retardancy and a preparation method thereof. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention aims to provide a composite barrier film with flame retardancy and a preparation method thereof. On the premise of improving the flame retardancy of the PET film, the composite film also has excellent heat sealing properties.

[0006] To achieve the above object, the present invention proposes the following technical solutions:

[0007] A flame-retardant composite barrier film, wherein the composite barrier film is made by directly co-extruding a flame-retardant PET film layer and a heat-sealing PP film layer;

[0008] Wherein, the flame retardant PET film layer is made of the following raw materials in parts by weight:

[0009]

[0010] The heat-sealed PP film layer is made of the following raw materials in parts by weight:

[0011]

[0012] Furthermore, the melt index of the modified PET resin is 13-15 g / 10 min, and the modified PET resin is obtained by being impregnated with an aminopropyltriethoxysilane solution and then dried to a moisture content of less than 0.2 wt%.

[0013] Furthermore, the aminopropyltriethoxysilane solution is prepared by mixing aminopropyltriethoxysilane and water in a volume ratio of (1-5):100.

[0014] Furthermore, the coated nano flame retardant is a nano alumina coated red phosphorus flame retardant.

[0015] Furthermore, the preparation method of the nano-alumina-coated red phosphorus flame retardant specifically comprises the following steps:

[0016] (1) placing red phosphorus in a planetary ball mill for ball milling at a rotation speed of 400 rpm, with a mass ratio of red phosphorus to distilled water of 1:35; adding water to the red phosphorus after the first ball milling to disperse it, allowing it to settle and separate to obtain a precipitate, and then ball milling it again to obtain ultrafine red phosphorus, and drying the ultrafine red phosphorus to a moisture content of less than 0.2 wt %;

[0017] (2) uniformly mixing the dried ultrafine red phosphorus and polyvinyl pyrrolidone in a mass ratio of 1:20 to obtain a mixed material A;

[0018] (3) taking aluminum isopropoxide and deionized water in a molar ratio of 1:1000, mixing them evenly, heating to 85° C., stirring for reaction for 1 hour, and cooling to room temperature; then adding the mixed material A in step (2), wherein the amount of red phosphorus used is 0.01 mol, calculated based on the amount of red phosphorus, to obtain a mixed material B;

[0019] (4) The mixed material B is ultrasonically dispersed for 0.5-1 h, and then a 50% by mass aqueous ammonia solution is added dropwise to adjust the pH to 9, and then filtered, washed, and dried to obtain a nano-alumina-coated red phosphorus flame retardant.

[0020] Furthermore, the method for preparing the flame-retardant composite barrier film comprises the following steps:

[0021] S1. Weigh the raw materials of the flame-retardant PET film layer and the heat-sealing PP film layer respectively by weight and set aside;

[0022] S2, preparing a mixture of the flame retardant PET film layer raw materials:

[0023] 1) drying the modified PET resin, polyacrylic acid resin, coated nano flame retardant and nano zinc oxide until the moisture content is less than 0.2wt%;

[0024] 2) Then the dried modified PET resin is placed on a flat substrate, and the toluene solution of MDI is sprayed on the surface of the modified PET resin, and after drying, it is mixed evenly with polyacrylic acid resin, coated nano flame retardant, and nano zinc oxide, and placed at 52-60° C. and 2-3 standard atmospheric pressures for 6-10 hours to obtain premix A;

[0025] 3) feeding the premix A into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a flame-retardant PET film layer melt;

[0026] S3, preparing a mixture of the raw materials for the heat-sealed PP film layer:

[0027] 1) drying random copolymerized polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate until the moisture content is less than 0.2 wt %;

[0028] 2) then uniformly mixing the dried random copolymer polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate to obtain a premix B;

[0029] 3) The premix B is fed into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a heat-sealing PP film layer melt;

[0030] S4, the flame-retardant PET film layer melt and the heat-sealing PP film layer melt are combined at the die head and then extruded, and are rapidly cooled by a cooling roller and a water tank to form a solid casting sheet;

[0031] S5, then longitudinal stretching is performed, the longitudinal stretching temperature is 95-105°C, and the longitudinal stretching multiple is 5-7 times;

[0032] S6, then transverse stretching is performed, the transverse stretching temperature is 105-125°C, and the transverse stretching multiple is 6-9 times; cooling and shaping treatment is performed immediately after stretching, and the cold air temperature is 20-30°C;

[0033] S7, and then sequentially undergoing online thickness measurement, edge material cutting, automatic winding, aging treatment, and finally slitting to obtain the finished composite barrier film.

[0034] Furthermore, the thickness of the composite barrier film is 50-75 um.

[0035] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0036] The present invention discloses a composite barrier film with flame retardancy and a preparation method thereof. The composite barrier film is made by directly co-extruding a flame retardant PET film layer and a heat-sealing PP film layer, which can not only maintain the excellent heat-sealing performance of the PP film, but also further enhance the flame retardant effect of the composite film. The PET resin used in the flame retardant PET film layer is amino-treated, and the network structure formed by the combined use of MDI and polyacrylic acid resin is more compact, which enhances the barrier performance of the composite film and also helps flame retardancy to a certain extent; the further filling of the coated nano flame retardant and nano zinc oxide improves the mechanical properties of the film and enhances the flame retardant effect, and the increase in density is also beneficial to the barrier effect of oxygen and the like. The PP film layer is not only a guarantee of heat sealing performance, but the addition of zinc metaborate enhances the film compatibility and helps the composite film to form a three-dimensional network structure, and the structural stability of the composite film is good. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0038] The words "first", "second" and similar words used in the patent application specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, unless the context clearly indicates otherwise, the singular forms of "a", "an" or "the" and other similar words do not indicate a quantitative limitation, but indicate the existence of at least one. Words such as "include" or "comprise" mean that the elements or objects appearing before "include" or "comprise" cover the features, wholes, steps, operations, elements and / or components listed after "include" or "comprise", and do not exclude the existence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0039] In the present invention, the coated nano flame retardant is a nano alumina-coated red phosphorus flame retardant. Further, the preparation method of the nano alumina-coated red phosphorus flame retardant specifically comprises the following steps:

[0040] (1) placing red phosphorus in a planetary ball mill for ball milling at a rotation speed of 400 rpm, with a mass ratio of red phosphorus to distilled water of 1:35; adding water to the red phosphorus after the first ball milling to disperse it, allowing it to settle and separate to obtain a precipitate, and then ball milling it again to obtain ultrafine red phosphorus, and drying the ultrafine red phosphorus to a moisture content of less than 0.2 wt %;

[0041] (2) uniformly mixing the dried ultrafine red phosphorus and polyvinyl pyrrolidone in a mass ratio of 1:20 to obtain a mixed material A;

[0042] (3) taking aluminum isopropoxide and deionized water in a molar ratio of 1:1000, mixing them evenly, heating to 85° C., stirring for reaction for 1 hour, and cooling to room temperature; then adding the mixed material A in step (2), wherein the amount of red phosphorus used is 0.01 mol, calculated based on the amount of red phosphorus, to obtain a mixed material B;

[0043] (4) The mixed material B is ultrasonically dispersed for 0.5-1 h, and then a 50% by mass aqueous ammonia solution is added dropwise to adjust the pH to 9, and then filtered, washed, and dried to obtain a nano-alumina-coated red phosphorus flame retardant.

[0044] Red phosphorus is a traditional and highly effective halogen-free flame retardant. However, the main disadvantages of red phosphorus are that it reacts with water vapor in the air to produce highly toxic phosphine, poor thermal stability, and lack of compatibility with synthetic resins, which also affects its use. The current method to improve the stability of red phosphorus is to encapsulate the surface of red phosphorus powder with organic and inorganic substances to form microencapsulated red phosphorus to isolate moisture. Microencapsulated red phosphorus has high moisture resistance, good fluidity, can prolong storage time and reduce the formation of phosphine. In the preparation process of microencapsulated red phosphorus, suitable shell material is an important factor in determining flame retardant properties.

[0045] In the coated nano flame retardant, red phosphorus intercepts free radicals, improves thermal stability, and is stably combined with nano alumina. Red phosphorus reacts with oxygen to form phosphorus oxygen groups, which continue to react with polymers to produce cross-linked structures to obtain a phosphorus-oxygen cross-linked carbonized layer; it reacts with oxygen in the environment to generate oxygen-containing phosphates, which have strong hygroscopicity and can reduce the surface temperature of the burning polymer, while promoting the surface humidity of the polymer and the surface carbonization of the polymer; nano alumina is more likely to decompose at high temperatures to produce aluminum oxide smoke, forming a flame retardant layer, which plays a role in isolating air and burning substances. The combination of coated nano flame retardants has a flame retardant synergistic effect. The present invention uses nano alumina as a shell material, which not only has a flame retardant synergistic effect with red phosphorus, but can also be stably coated on the outer surface of red phosphorus while nano alumina is formed.

[0046] Further, the modified PET resin of the present invention is dried to a moisture content of less than 0.2wt% after being impregnated with an aminopropyl triethoxysilane solution. The specific treatment is to configure the aminopropyl triethoxysilane solution and water into a solution at a volume ratio of 1:100, and immerse the PET resin in the aqueous solution for more than 24 hours, so that the PET surface has active amino groups. Further, the modified PET resin is placed on a flat substrate, and a toluene solution of MDI (4,4'-diphenylmethane diisocyanate) is sprayed on the surface of the modified PET resin, so that the amino group and the isocyanate group of MDI undergo a substitution reaction, and then the PET surface forms a large steric modified polymer with an isocyanate group through a uric acid bond. It is mixed evenly with the dried polyacrylic resin, the coated nano flame retardant, and the nano zinc oxide, and placed at 60°C and 2 standard atmospheric pressures for 7 hours to obtain a premix A, so that the isocyanate group on the PET surface reacts with the carboxyl group on the polyacrylic resin to obtain a two-dimensional network structure. Encapsulated nano flame retardants, nano zinc oxide, etc. can be filled into the mesh gaps, so that when the encapsulated nano flame retardants and nano zinc oxide play a flame retardant effect, the dense network structure can also play a barrier role.

[0047] Furthermore, the use of copolymers in the heat-sealed PP film layer can play a role in the transition of the double-layer composite film, ensuring the compatibility and overall stability of the film as a whole, and the zinc metaborate therein is an environmentally friendly non-halogen flame retardant, non-toxic, low water solubility, high thermal stability, small particle size, small specific gravity, good dispersibility, etc. As a high-efficiency flame retardant, it is widely used in the fields of plastics, rubber, coatings, etc. Further, the zinc metaborate is placed in a hot alkaline solution and stirred for 0.5 hours before use, and dried in a 60°C forced air drying oven to a moisture content of less than 0.2wt%, and then used immediately. This is to allow zinc metaborate to form metaborate in an alkaline solution. During the composite film forming process, the metaborate can undergo an esterification reaction with the carboxyl functional group in the polyacrylic acid resin. First, the chemical bonds formed by the functional groups are used to enhance the stability of the composite film. Second, the use of zinc metaborate allows the polyacrylic acid to form a cross-linked network. Coupled with the combination of a flame-retardant PET film layer, the composite film is denser and the network structure is tighter, thereby enhancing the oxygen barrier effect and thereby improving the film barrier properties.

[0048] Performance Testing

[0049] Mechanical properties test

[0050] According to GB / T 1040.3-2006 standard, multiple samples in the same group were tested and the average value was taken to obtain the tensile strength of the film.

[0051] Heat seal strength test

[0052] The heat seal strength test of plastic film refers to the standard QB / T2358-2009 "Plastic Film Packaging Bag Heat Seal Strength Test_Test_Specimen_Fixture". The test sample is prepared according to the test requirements and the average value is taken after three tests.

[0053] Barrier performance test

[0054] The barrier performance test of the film includes water vapor barrier performance, which can be converted by water vapor transmission rate. Water vapor transmission rate can be directly tested using the WVTR-RC6 water vapor transmission rate tester of Shandong Puchuang Industrial Technology Co., Ltd. The test method is not repeated here. Water vapor transmission rate is an important indicator for evaluating the moisture resistance of composite films. The unit of water vapor transmission rate is The test results are expressed as the arithmetic mean of three samples. The greater the water vapor transmission rate, the worse the water vapor barrier performance.

[0055] The barrier performance test of the film includes the oxygen barrier performance test. The test standard refers to the gas permeation rate determination method (YBB00082003-2015). The sample preparation requirements are all specified in the standard and will not be repeated here. In the oxygen barrier performance test, the unit of oxygen permeation rate is Take at least five points for measurement and take the arithmetic mean.

[0056] Flame retardant

[0057] The flame retardant performance test of the film is carried out according to the ANSL-UL94-2009 "Vertical and Horizontal Burning Tester_Performance_Plastics_Test" standard. The test thickness of the film is further hot-pressed to meet the test requirements, and then the flame retardant performance is tested and evaluated.

[0058] Examples 1-3

[0059] A flame-retardant composite barrier film is prepared by direct co-extrusion of a flame-retardant PET film layer and a heat-sealed PP film layer. The components shown in Table 1 are weighed by weight percentage and then prepared according to the following steps:

[0060] S1. Weigh the raw materials of the flame-retardant PET film layer and the heat-sealing PP film layer respectively by weight and set aside;

[0061] S2, preparing a mixture of the flame retardant PET film layer raw materials:

[0062] 1) drying the modified PET resin, polyacrylic acid resin, coated nano flame retardant and nano zinc oxide until the moisture content is less than 0.2wt%;

[0063] 2) Then the dried modified PET resin is placed on a flat substrate, and the toluene solution of MDI is sprayed on the surface of the modified PET resin, and after drying, it is mixed evenly with polyacrylic acid resin, coated nano flame retardant, and nano zinc oxide, and placed at 52-60° C. and 2-3 standard atmospheric pressures for 6-10 hours to obtain premix A;

[0064] 3) feeding the premix A into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a flame-retardant PET film layer melt;

[0065] S3, preparing a mixture of the raw materials for the heat-sealed PP film layer:

[0066] 1) drying random copolymerized polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate until the moisture content is less than 0.2 wt %;

[0067] 2) then uniformly mixing the dried random copolymer polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate to obtain a premix B;

[0068] 3) The premix B is fed into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a heat-sealing PP film layer melt;

[0069] S4, the flame-retardant PET film layer melt and the heat-sealing PP film layer melt are combined at the die head and then extruded, and are rapidly cooled by a cooling roller and a water tank to form a solid casting sheet;

[0070] S5, then longitudinal stretching is performed, the longitudinal stretching temperature is 95-105°C, and the longitudinal stretching multiple is 5-7 times;

[0071] S6, then transverse stretching is performed, the transverse stretching temperature is 105-125°C, and the transverse stretching multiple is 6-9 times; cooling and shaping treatment is performed immediately after stretching, and the cold air temperature is 20-30°C;

[0072] S7, and then sequentially undergoing online thickness measurement, edge material cutting, automatic winding, aging treatment, and finally slitting to obtain the finished composite barrier film.

[0073] Preferably, in order to make the composite film have good mechanical strength and composite stability, and according to the preparation characteristics of polypropylene film, we use a biaxial stretching process to improve the composite of the heat-sealed PP film layer and the flame-retardant PET film layer. Among them, the longitudinal stretching temperature of step S5 is 105°C, and the longitudinal stretching multiple is 6 times; the transverse stretching temperature of step S6 is 105°C, and the transverse stretching multiple is 6 times; after stretching, cooling and shaping treatment is immediately carried out, and the cold air temperature is 20°C.

[0074] In the present invention, in order to ensure the flame retardancy of the composite film, a coated nano flame retardant is used, specifically a nano alumina-coated red phosphorus flame retardant. The preparation method of the nano alumina-coated red phosphorus flame retardant specifically comprises the following steps:

[0075] (1) placing red phosphorus in a planetary ball mill for ball milling at a rotation speed of 400 rpm, with a mass ratio of red phosphorus to distilled water of 1:35; adding water to the red phosphorus after the first ball milling to disperse it, allowing it to settle and separate to obtain a precipitate, and then ball milling it again to obtain ultrafine red phosphorus, and drying the ultrafine red phosphorus to a moisture content of less than 0.2 wt %;

[0076] (2) uniformly mixing the dried ultrafine red phosphorus and polyvinyl pyrrolidone in a mass ratio of 1:20 to obtain a mixed material A;

[0077] (3) taking aluminum isopropoxide and deionized water in a molar ratio of 1:1000, mixing them evenly, heating to 85° C., stirring for reaction for 1 hour, and cooling to room temperature; then adding the mixed material A in step (2), wherein the amount of red phosphorus used is 0.01 mol, calculated based on the amount of red phosphorus, to obtain a mixed material B;

[0078] (4) The mixed material B is ultrasonically dispersed for 0.5-1 h, and then a 50% by mass aqueous ammonia solution is added dropwise to adjust the pH to 9, and then filtered, washed, and dried to obtain a nano-alumina-coated red phosphorus flame retardant.

[0079] Furthermore, in the embodiment, in order to ensure the compatibility between the materials, the modified PET resin in the flame-retardant PET film layer is dried to a moisture content of less than 0.2wt% after being impregnated with an aminopropyltriethoxysilane solution. Furthermore, the aminopropyltriethoxysilane solution is prepared by mixing aminopropyltriethoxysilane and water in a volume ratio of 1:100. Furthermore, the PET resin is immersed in an aqueous solution of aminopropyltriethoxysilane for 36 hours. Furthermore, the modified PET resin is placed on a flat substrate, and the toluene solution of MDI is sprayed on the surface of the modified PET resin. At the same time, the modified PET resin on the substrate is evenly tumbled using equipment such as a shaking table, so that the toluene solution of MDI is evenly sprayed on the surface of the modified PET resin, and then dried to a moisture content of less than 0.2wt%.

[0080] Furthermore, the nano zinc oxide powder was purchased from Wuhan Kemik Biomedical Technology Co., Ltd.; and the MDI was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0081] In the present invention, the thickness of the PET film is 55 um.

[0082] Comparative Example 1

[0083] A common heat-sealable PET film was purchased from the market. The film-making process was the same as that in Example 1, and the specification parameters were the same as those in Example 1.

[0084] Comparative Example 2

[0085] A commercially available common heat-sealable PP film was purchased. The film-making process was the same as that of Example 1, and the specification parameters thereof were referenced to Example 1.

[0086] Comparative Example 3

[0087] The difference from Example 1 is that the modified PET resin of the flame-retardant PET film layer is replaced by a PET resin that has not been treated with aminopropyltriethoxysilane solution. The other process and technical parameters refer to Example 1.

[0088] Comparative Examples 4-6

[0089] The difference from Example 1 is that the components shown in Table 1 are weighed by weight percentage, and other process and technical parameters refer to Example 1.

[0090] The samples were prepared according to relevant test standards. The thickness of the composite barrier films of the present invention was 55 um. The relevant test comparisons are shown in Table 1.

[0091] Table 1 Material ratio and test results analysis table

[0092]

[0093] From the analysis of the comparison results in Table 1 above, it can be seen that from the perspective of flame retardancy, the lack of the coated nano flame retardant in Comparative Example 6 has a greater impact on the flame retardant effect of the composite film. The non-use of zinc metaborate in Comparative Example 5 will have an impact on flame retardancy because there will be an esterification reaction between the metaborate structure and the carboxyl group on the polyacrylic acid, so that the composite film forms a three-dimensional structure and a denser network, which in turn affects the barrier properties and also has a certain impact on flame retardancy. In terms of barrier properties, the surface amination of the PET resin in Comparative Example 3 affects the bond energy bonding, so the density between the chain segments decreases, the intermolecular gap is larger, resulting in a decrease in its barrier properties, and a significant impact on its mechanical strength. Due to the lack of polyacrylic acid in Comparative Example 4, similarly, the intermolecular bonding is weakened, the density decreases, and the mechanical properties are sharply reduced.

[0094] In summary, the composite barrier film of the present application is flame retardant V0 grade and is a packaging material with excellent flame retardant properties. It has the characteristics of high flame retardant temperature, good self-extinguishing performance, excellent barrier properties and excellent mechanical properties, and has broad application prospects.

[0095] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A flame retardant composite barrier film, It is characterized in that The composite barrier film is made by direct co-extrusion of a flame-retardant PET film layer and a heat-sealing PP film layer; Wherein, the flame retardant PET film layer is made of the following raw materials in parts by weight: The heat-sealed PP film layer is made of the following raw materials in parts by weight:

2. The flame retardant composite barrier film according to claim 1, It is characterized in that The melt index of the modified PET resin is 13-15 g / 10 min, and the modified PET resin is obtained by being impregnated with an aminopropyltriethoxysilane solution and then dried until the moisture content is less than 0.2 wt%.

3. The flame retardant composite barrier film according to claim 2, It is characterized in that The aminopropyltriethoxysilane solution is prepared by mixing aminopropyltriethoxysilane and water in a volume ratio of (1-5):

100.

4. The flame retardant composite barrier film according to claim 1, It is characterized in that The coated nano flame retardant is a nano alumina coated red phosphorus flame retardant.

5. The flame retardant composite barrier film according to claim 4, It is characterized in that The preparation method of the nano-alumina-coated red phosphorus flame retardant specifically comprises the following steps: (1) placing red phosphorus in a planetary ball mill for ball milling at a rotation speed of 400 rpm, with a mass ratio of red phosphorus to distilled water of 1:35; adding water to the red phosphorus after the first ball milling to disperse it, allowing it to settle and separate to obtain a precipitate, and then ball milling it again to obtain ultrafine red phosphorus, and drying the ultrafine red phosphorus to a moisture content of less than 0.2 wt %; (2) uniformly mixing the dried ultrafine red phosphorus and polyvinyl pyrrolidone in a mass ratio of 1:20 to obtain a mixed material A; (3) taking aluminum isopropoxide and deionized water in a molar ratio of 1:1000, mixing them evenly, heating to 85° C., stirring for reaction for 1 hour, and cooling to room temperature; then adding the mixed material A in step (2), wherein the amount of red phosphorus used is 0.01 mol, calculated based on the amount of red phosphorus, to obtain a mixed material B; (4) The mixed material B is ultrasonically dispersed for 0.5-1 h, and then a 50% by mass aqueous ammonia solution is added dropwise to adjust the pH to 9, and then filtered, washed, and dried to obtain a nano-alumina-coated red phosphorus flame retardant.

6. A method for preparing a flame-retardant composite barrier film according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1. Weigh the raw materials of the flame-retardant PET film layer and the heat-sealing PP film layer respectively by weight and set aside; S2, preparing a mixture of the flame retardant PET film layer raw materials: 1) drying the modified PET resin, polyacrylic acid resin, coated nano flame retardant and nano zinc oxide until the moisture content is less than 0.2wt%; 2) Then the dried modified PET resin is placed on a flat substrate, and the toluene solution of MDI is sprayed on the surface of the modified PET resin, and after drying, it is mixed evenly with polyacrylic acid resin, coated nano flame retardant, and nano zinc oxide, and placed at 52-60° C. and 2-3 standard atmospheric pressures for 6-10 hours to obtain premix A; 3) feeding the premix A into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a flame-retardant PET film layer melt; S3, preparing a mixture of the raw materials for the heat-sealed PP film layer: 1) drying random copolymerized polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate until the moisture content is less than 0.2 wt %; 2) then uniformly mixing the dried random copolymer polypropylene, ethylene-methyl acrylate copolymer, propylene-ethylene copolymer, and zinc metaborate to obtain a premix B; 3) The premix B is fed into a melting twin-screw extruder and a metering twin-screw extruder connected in series for melting and plasticization to form a heat-sealing PP film layer melt; S4, the flame-retardant PET film layer melt and the heat-sealing PP film layer melt are combined at the die head and then extruded, and are rapidly cooled by a cooling roller and a water tank to form a solid casting sheet; S5, then longitudinal stretching is performed, the longitudinal stretching temperature is 95-105°C, and the longitudinal stretching multiple is 5-7 times; S6, then transverse stretching is performed, the transverse stretching temperature is 105-125°C, and the transverse stretching multiple is 6-9 times; cooling and shaping treatment is performed immediately after stretching, and the cold air temperature is 20-30°C; S7, and then sequentially undergoing online thickness measurement, edge material cutting, automatic winding, aging treatment, and finally slitting to obtain the finished composite barrier film.

7. The method for preparing a flame-retardant composite barrier film according to claim 7, It is characterized in that The thickness of the composite barrier film is 50-75 um.

Citation Information

Patent Citations

  • High barrier PET / PP film

    CN106117527A

  • heat-sealing BOPP film for cigarettes and preparation method of BOPP film

    CN113059880A

  • Efficient PP flame-retardant master batch and preparation method thereof

    CN113248831A

  • Antistatic antibacterial biaxially oriented polyester composite film and preparation method thereof

    CN116655983A

  • Thermoplastic resin pultrusion composite material and processing technology thereof

    CN117965002A