Laminated and printed non-woven fabric

By designing a combination of multi-layer structures and specific fiber materials in non-woven fabrics, combining film printing and waterproof and vapor-permeable layer, the problems of taking into account both strength and aesthetics of the non-woven fabrics are solved, and high durability, model retention, corrosion resistance and Beautiful effect.

CN118952807APending Publication Date: 2024-11-15JIANGYIN ZHONGXING NON WOVEN FABRIC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411170590.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing non-woven fabrics are difficult to meet the growing requirements for strength and toughness, while aesthetics and functional requirements are difficult to take into account.

Method used

A film-printed non-woven fabric was designed, using a multi-layer structure including a high-strength antibacterial layer, a fluffy mold-retaining layer and a corrosion-resistant layer. It is designed by a film-printed layer and a waterproof and vapor-permeable layer, combined with spiral curled polyester fibers, Materials such as low-melting point polyester fiber, basalt fiber and carbon fiber are formed by hydrospuncture reinforcement and hot pressing.

Benefits of technology

The high durability, type retention, corrosion resistance and aesthetics of non-woven fabrics are achieved, which enhances its practicality, while reducing static electricity using the conductive properties of carbon fibers and ensuring waterproof and vapor permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118952807A_ABST
    Figure CN118952807A_ABST
Patent Text Reader

Abstract

The invention relates to a lamination printing non-woven fabric which comprises a non-woven fabric body (1), the non-woven fabric body (1) comprises a high-strength antibacterial layer (11), a fluffy shape-keeping layer (12) and a corrosion-resistant layer (13), the high-strength antibacterial layer (11) is arranged at the upper end of the fluffy shape-keeping layer (12), and the corrosion-resistant layer (13) is arranged at the lower end of the fluffy shape-keeping layer (12); the upper end of the high-strength antibacterial layer (11) is provided with a lamination printing layer (2), and the lower end of the corrosion-resistant layer (13) is provided with a waterproof vapor-permeable layer (3); the high-strength antibacterial layer (11), the fluffy shape-keeping layer (12) and the corrosion-resistant layer (13) are stacked and laid according to a preset structure, and are sequentially subjected to spunlace reinforcement, hot pressing treatment and rolling to form the non-woven fabric main body (1); through the design of the non-woven fabric main body structure and other functional layers, the prepared lamination printed non-woven fabric not only has aesthetic property and practicability, but also has excellent functionality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonwoven fabrics, and in particular relates to a laminated printed nonwoven fabric. Background Art

[0002] Non-woven fabric is a kind of fabric that does not require spinning and weaving. It is composed of directional or random fibers. It is a new generation of environmentally friendly materials. It has the characteristics of moisture-proof, breathable, flexible, lightweight, easy to decompose, non-toxic and non-irritating, rich colors, low price, and recyclable. The application field of non-woven fabric is very wide, mainly used in medical protection, clothing, home decoration, industrial fabrics and agricultural fields. The non-woven fabrics in the existing technology have good bonding or entanglement, and the strength and toughness are difficult to meet people's growing use requirements.

[0003] Laminating is an important process for the production of functional non-woven fabrics. It uses a laminating device to melt plastic and then sprinkle it on the surface of the non-woven fabric. It has the advantages of fast production speed, meeting customized needs, and more beautiful appearance. Therefore, designing a non-woven fabric that can meet both aesthetic needs and functionality for daily use is the current direction of non-woven fabric design. Summary of the invention

[0004] The purpose of the present invention is to provide a laminated printed nonwoven fabric in view of the above-mentioned prior art. Through the design of the nonwoven fabric main structure and other functional layers, the prepared laminated printed nonwoven fabric is not only aesthetically pleasing and practical, but also has excellent functionality.

[0005] The technical solution adopted by the present invention to solve the above problems is: a coated printed non-woven fabric, comprising a non-woven fabric body, the non-woven fabric body comprising a high-strength antibacterial layer, a fluffy shape-retaining layer and a corrosion-resistant layer, the high-strength antibacterial layer is arranged on the upper end of the fluffy shape-retaining layer, and the corrosion-resistant layer is arranged on the lower end; the coated printing layer is arranged on the upper end of the high-strength antibacterial layer, and the waterproof and breathable layer is arranged on the lower end of the corrosion-resistant layer; the high-strength antibacterial layer is a mixture of 50% by weight of antibacterial polyester fiber, 30% by weight of polyester-based graphene fiber and 20% by weight of ultra-high molecular weight polyethylene fiber, which are mixed, opened and The fluffy shape-retaining layer is a cotton net formed by mixing, loosening, combing and cross-laminating spiral curled polyester fibers with a weight ratio of 80% and low-melting point polyester fibers with a weight ratio of 20% to form a cotton net; the corrosion-resistant layer is a cotton net formed by mixing, loosening, combing and cross-laminating basalt fibers with a weight ratio of 50% and carbon fibers with a weight ratio of 50% to form a cotton net; the high-strength antibacterial layer, the fluffy shape-retaining layer and the corrosion-resistant layer are stacked in a preset structure, and are successively reinforced with water spunlace, hot-pressed and rolled up to form a non-woven fabric body.

[0006] The multi-layer setting of the non-woven fabric body gives it multiple functions, such as: the combination of the high-strength antibacterial layer and the corrosion-resistant layer can ensure that the non-woven fabric body has good durability; the design of the fluffy shape-keeping layer ensures that the non-woven fabric body has good shape-keeping performance; in the fluffy shape-keeping layer, spiral curled polyester fiber is used to ensure the fluffy resilience of the non-woven fabric body, and low-melting point polyester fiber is used to ensure the stability of the fluffy shape-keeping layer. The corrosion-resistant layer uses basalt fiber and carbon fiber mixed fiber with excellent corrosion resistance, which not only ensures that the non-woven fabric body has excellent corrosion resistance, but also enables the non-woven fabric body to use the conductive properties of carbon fiber to reduce static electricity in the non-woven fabric body.

[0007] Furthermore, the method for preparing the laminated printing layer comprises the following steps:

[0008] I. Material collection: according to mass fraction, take 70-80 parts of LLDPE particles, 10-15 parts of LDPE particles, and 10-15 parts of adhesive particles;

[0009] II. Pretreatment: Mix LLDPE particles and LDPE particles in an internal mixer at 80°C for 10 minutes at a speed of 30r / min. Take them out after the torque reaches the equilibrium point, cool them down, and place them in a drying container for later use;

[0010] III. Mixing and melting: The pretreated material is mixed with adhesive particles, and the particles are melted by heating and stirring. The adhesive particles are multi-layer co-extruded film adhesive particles, which are obtained by chemically connecting maleic anhydride polar groups to polyethylene molecular chains to form modified polyethylene, and then the modified polyethylene is made into particles by granulation equipment. Since the polar groups of maleic anhydride are re-reactive, high adhesion to PE materials can be achieved. The heating temperature during melting is 120-125°C.

[0011] IV. Filtration: Filter the molten solution through a filter with a precision of 20um;

[0012] V. Laminating and printing: The filtered solution is sprayed onto the upper surface of the high-strength antibacterial layer through the membrane head of the laminating machine to form a liquid film; then the pigment is quickly sprayed onto the surface of the liquid film through the printing nozzle in a certain pattern to form a liquid film with a certain pattern;

[0013] VI. After the non-woven fabric body after forming the liquid film passes through the cooling and drying equipment, a dense printed film is formed on the surface of the high-strength antibacterial layer;

[0014] The setting of the laminating printing layer not only has a certain protective effect on the non-woven fabric body, but also utilizes the printing on the surface of the laminating film to increase the aesthetics of the non-woven fabric and make the non-woven fabric more practical; the laminating printing layer closely combines the laminating film and the printing, and fixes the pigment through the viscosity of the film layer after laminating, so that the pigment and the film layer are fully combined, thereby ensuring the integrity of the printing film and the firmness of the pattern.

[0015] Furthermore, the waterproof and vapor-permeable layer is a modified LDPE waterproof and vapor-permeable film, and its specific preparation method is: irradiating the LDPE dry film with a Co-60γ source to generate carboxyl groups on the LDPE molecular chain, and then using polyvinyl alcohol to combine with the carboxyl groups on the molecular chain, thereby grafting the polyvinyl alcohol onto the LDPE film. The hydrophilic property of polyvinyl alcohol makes the modified LDPE have the property that water droplets cannot penetrate but water vapor can pass freely, so that the non-woven fabric is not only waterproof but also has good vapor permeability.

[0016] Furthermore, the modified LDPE waterproof vapor-permeable membrane is point-bonded to the corrosion-resistant layer to form a waterproof vapor-permeable layer; the point bonding avoids insufficient vapor permeability caused by full bonding, which affects the performance of the waterproof vapor-permeable layer and increases the corrosion rate of the material.

[0017] Furthermore, the thickness of the high-strength antibacterial layer, the fluffy shape-retaining layer and the corrosion-resistant layer are all 100-120 um.

[0018] Compared with the prior art, the nonwoven fabric of the present invention has the following advantages: (1) The provision of the laminated printing layer not only has a certain protective effect on the nonwoven fabric body, but also utilizes the printing on the surface of the laminated film to increase the aesthetics of the nonwoven fabric, making the nonwoven fabric more practical; the laminated printing layer closely combines the laminated film and the printing, and fixes the pigment through the viscosity of the film layer after the laminated film, so that the pigment and the film layer are fully combined, thereby ensuring the integrity of the printing film and the firmness of the pattern. (2) The multi-layer setting of the non-woven fabric body makes it have multiple functions; the combination of the high-strength antibacterial layer and the corrosion-resistant layer can ensure that the non-woven fabric body has good durability; the design of the fluffy shape-retaining layer ensures that the non-woven fabric body has good shape-retaining performance; in the fluffy shape-retaining layer, spiral curled polyester fiber is used to ensure the fluffy resilience of the non-woven fabric body, and low-melting point polyester fiber is used to ensure the stability of the fluffy shape-retaining layer; the corrosion-resistant layer uses basalt fiber and carbon fiber mixed fiber with excellent corrosion resistance, which not only ensures that the non-woven fabric body has excellent corrosion resistance, but also enables the non-woven fabric body to use the conductive properties of carbon fiber to reduce the static electricity of the non-woven fabric body. (3) The modified LDPE waterproof and breathable film used in the waterproof and breathable layer makes the non-woven fabric not only waterproof, but also has good breathability. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the structure of the fabric in the embodiment of the present invention

[0020] In the figure: 1. Fabric body; 2. Laminated printing layer; 3. Waterproof and breathable layer; 11. High-strength antibacterial layer; 12. Fluffy shape-retaining layer; 13. Corrosion-resistant layer; DETAILED DESCRIPTION

[0021] The present invention is further described in detail below with reference to the accompanying drawings.

[0022] like Figure 1 As shown, the coated printed non-woven fabric of this embodiment comprises a non-woven fabric body 1, wherein the non-woven fabric body 1 comprises a high-strength antibacterial layer 11, a fluffy shape-retaining layer 12 and a corrosion-resistant layer 13, wherein the high-strength antibacterial layer 11 is arranged on the upper end of the fluffy shape-retaining layer 12, and the corrosion-resistant layer 13 is arranged on the lower end; a coated printing layer 2 is arranged on the upper end of the high-strength antibacterial layer 11, and a waterproof vapor-permeable layer 3 is arranged on the lower end of the corrosion-resistant layer 13; the high-strength antibacterial layer 11 is a cotton net formed by mixing, opening, combing and cross-laying antibacterial polyester fibers with a weight ratio of 50%, polyester-based graphene fibers with a weight ratio of 30% and ultra-high molecular weight polyethylene fibers with a weight ratio of 20%; the fluffy The shape-retaining layer 12 is a cotton net formed by mixing, loosening, combing and cross-laying spirally curled polyester fibers with a weight ratio of 80% and low-melting point polyester fibers with a weight ratio of 20%; the corrosion-resistant layer 13 is a cotton net formed by mixing, loosening, combing and cross-laying basalt fibers with a weight ratio of 50% and carbon fibers with a weight ratio of 50%; the high-strength antibacterial layer 11, the fluffy shape-retaining layer 12 and the corrosion-resistant layer 13 are stacked in a preset structure, and are successively reinforced with water spunlace, hot-pressed and rolled to form a non-woven fabric body 1; the thickness of the high-strength antibacterial layer 11, the fluffy shape-retaining layer 12 and the corrosion-resistant layer 13 are all 100-120um.

[0023] The multi-layer arrangement of the non-woven fabric body 1 enables it to have multiple functions, such as: the combination of the high-strength antibacterial layer 11 and the corrosion-resistant layer 13 can ensure that the non-woven fabric body 1 has good durability; the design of the fluffy shape-retaining layer 12 ensures that the non-woven fabric body has good shape-retaining performance; in the fluffy shape-retaining layer 12, spirally curled polyester fibers are used to ensure the fluffy resilience of the non-woven fabric body 1, and low-melting point polyester fibers are used to ensure the stability of the fluffy shape-retaining layer 12. The corrosion-resistant layer 13 uses basalt fibers and carbon fiber mixed fibers with excellent corrosion resistance, which not only ensures that the non-woven fabric body has excellent corrosion resistance, but also enables the non-woven fabric body 1 to use the conductive properties of carbon fibers to reduce static electricity in the non-woven fabric body.

[0024] The preparation method of the laminated printing layer 2 comprises the following steps:

[0025] I. Material collection: According to the mass fraction, take 70 parts of LLDPE particles, 15 parts of LDPE particles, and 15 parts of adhesive particles;

[0026] II. Pretreatment: Mix LLDPE particles and LDPE particles in an internal mixer at 80°C for 10 minutes at a speed of 30r / min. Take them out after the torque reaches the equilibrium point, cool them down, and place them in a drying container for later use;

[0027] III. Mixing and melting: The pretreated material is mixed with adhesive particles, and the particles are melted by heating and stirring. The adhesive particles are multi-layer co-extruded film adhesive particles, which are obtained by chemically connecting maleic anhydride polar groups to polyethylene molecular chains to form modified polyethylene, and then the modified polyethylene is made into particles by granulation equipment. Since the polar groups of maleic anhydride are re-reactive, high adhesion to PE materials can be achieved. The heating temperature during melting is 120-125°C.

[0028] IV. Filtration: Filter the molten solution through a filter with a precision of 20um;

[0029] V. Laminating and printing: The filtered solution is sprayed onto the upper surface of the high-strength antibacterial layer 11 through the film head of the laminating machine to form a liquid film; then the pigment is quickly sprayed onto the surface of the liquid film through the printing nozzle in a certain pattern to form a liquid film with a certain pattern;

[0030] VI. After the non-woven fabric body 1 after forming the liquid film passes through a cooling and drying device, a dense printed film is formed on the high-strength antibacterial layer 11;

[0031] The setting of the laminated printing layer 2 not only has a certain protective effect on the non-woven fabric body 1, but also utilizes the printing on the surface of the laminated film to increase the aesthetics of the non-woven fabric and make the non-woven fabric more practical; the laminated printing layer 2 closely combines the laminated film and the printing, and fixes the pigment through the viscosity of the film layer after the laminated film, so that the pigment and the film layer are fully combined, thereby ensuring the integrity of the printing film and the firmness of the pattern.

[0032] The waterproof vapor-permeable layer 3 is a modified LDPE waterproof vapor-permeable film, which is point-bonded with the corrosion-resistant layer 13 to form the waterproof vapor-permeable layer 3; the specific preparation method of the modified LDPE waterproof vapor-permeable film is as follows: the LDPE dry film is irradiated with a Co-60γ source to generate carboxyl groups on the LDPE molecular chain, and then polyvinyl alcohol is combined with the carboxyl groups on the molecular chain to graft the polyvinyl alcohol onto the LDPE film. The hydrophilic property of polyvinyl alcohol makes the modified LDPE have the property that water droplets cannot penetrate but water vapor can pass freely, so that the non-woven fabric is not only waterproof but also has good vapor permeability.

[0033] In this embodiment, through the design of yarn structure, fabric component design, organizational structure design, and fabric dyeing and finishing process design, the prepared cashmere fabric is fluffy and soft, has a smooth surface, is warm and has little strength loss. It is not only cost-effective and has stable performance, but also has excellent functionality.

[0034] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A laminated printed nonwoven fabric, comprising a nonwoven fabric body (1), It is characterized in that The nonwoven fabric body (1) comprises a high-strength antibacterial layer (11), a fluffy shape-retaining layer (12) and a corrosion-resistant layer (13); the high-strength antibacterial layer (11) is arranged at the upper end of the fluffy shape-retaining layer (12), and the corrosion-resistant layer (13) is arranged at the lower end; the high-strength antibacterial layer (11) is arranged at the upper end of the film-coated printing layer (2), and the corrosion-resistant layer (13) is arranged at the lower end of the waterproof and breathable layer (3); the high-strength antibacterial layer (11) is a mixture of 50% by weight of antibacterial polyester fibers, 30% by weight of polyester-based graphene fibers and 20% by weight of ultra-high molecular weight polyethylene fibers, which are mixed, opened, combed and crossed. The fluffy shape-retaining layer (12) is a cotton net formed by mixing, opening, combing and cross-laying 80% by weight of spiral curled polyester fibers and 20% by weight of low melting point polyester fibers; the corrosion-resistant layer (13) is a cotton net formed by mixing, opening, combing and cross-laying 50% by weight of basalt fibers and 50% by weight of carbon fibers; the high-strength antibacterial layer (11), the fluffy shape-retaining layer (12) and the corrosion-resistant layer (13) are stacked in a preset structure, and are successively subjected to water spunlace reinforcement, hot pressing treatment and winding to form a non-woven fabric body (1).

2. The laminated printed nonwoven fabric according to claim 1, It is characterized in that The method for preparing the laminating printing layer (2) comprises the following steps: I. Material collection: according to mass fraction, take 70-80 parts of LLDPE particles, 10-15 parts of LDPE particles, and 10-15 parts of adhesive particles; II. Pretreatment: Mix LLDPE particles and LDPE particles in an internal mixer at 80°C for 10 minutes. The speed of the internal mixer is 30r / min. After the rotational torque reaches the equilibrium point, take out the particles, cool them, and place them in a drying container for later use. III. Mixing and melting: The pretreated material is mixed with adhesive particles, and the particles are melted by heating and stirring. The adhesive particles are multi-layer co-extruded film adhesive particles, which are obtained by chemically connecting maleic anhydride polar groups to polyethylene molecular chains to form modified polyethylene, and then the modified polyethylene is made into particles by granulation equipment. Since the polar groups of maleic anhydride are re-reactive, high adhesion to PE materials can be achieved. The heating temperature during melting is 120-125°C. IV. Filtration: Filter the molten solution through a filter with a precision of 20um; V. Laminating and printing: the filtered solution is sprayed onto the upper surface of the high-strength antibacterial layer (11) through the film head of the laminating machine to form a liquid film; then the pigment is quickly sprayed onto the surface of the liquid film in a certain pattern through the printing nozzle to form a liquid film with a certain pattern; VI. After the non-woven fabric body (1) with the liquid film formed thereon passes through a cooling and drying device, a dense printed film is formed on the high-strength antibacterial layer (11).

3. The laminated printed nonwoven fabric according to claim 1, It is characterized in that The waterproof vapor-permeable layer (3) is a modified LDPE waterproof vapor-permeable film, and its specific preparation method is: irradiating the LDPE dry film with a Co-60γ source to generate carboxyl groups on the LDPE molecular chain; then combining polyvinyl alcohol with the carboxyl groups on the molecular chain, thereby grafting the polyvinyl alcohol onto the LDPE film; the hydrophilic property of the polyvinyl alcohol enables the modified LDPE to have the property that water droplets cannot penetrate but water vapor can freely pass through.

4. The laminated printed nonwoven fabric according to claim 3, It is characterized in that The modified LDPE waterproof and vapor-permeable membrane is glued to the corrosion-resistant layer (13) in a dot-shaped manner to form a waterproof and vapor-permeable layer (3).

5. The laminated printed nonwoven fabric according to claim 1, It is characterized in that The thickness of the high-strength antibacterial layer (11), the fluffy shape-preserving layer (12) and the corrosion-resistant layer (13) are all 100-120 um.

Citation Information

Patent Citations

  • Manufacturing process of fluffy non-woven fabrics

    CN105002654A

  • Cutting-preventing gloves used during surgery and preparation method of cutting-preventing gloves

    CN110236687A

  • High-gloss and high-interlayer-fastness aluminum-plastic sheet and preparation method thereof

    CN115891354A

  • High-temperature-resistant corrosion-resistant environment-friendly filter material for filtration and preparation method thereof

    CN116371082A

  • Pre-irradiation grafting technoogical process of preparing antifogging polyethylene film

    CN1370795A