Method for improving compaction density of lithium iron phosphate positive electrode material of lithium ion battery

Through high-temperature drying, powder tableting and hydrothermal sintering, combined with metal ion doping and surface coating, nanospherical carbon-coated lithium iron phosphate positive electrode material is prepared, which solves the low compaction density and electrical conductivity of lithium iron phosphate positive electrode material. The problem of poor performance has achieved the improvement of high energy density and stability of the material.

CN118954460APending Publication Date: 2024-11-15SHENYANG INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411008236.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The compaction density of lithium iron phosphate cathode material is low, which limits its energy density and hinders its industrialization development. It also has problems such as low electronic conductivity and low lithium ion diffusion coefficient.

Method used

Through high-temperature drying, powder tableting, ball milling, hydrothermal sintering and other steps, combined with metal ion doping and surface coating, the morphological characteristics and particle size of the material are controlled, glucose and other carbon sources are used, and hexadecyl tritetrade is added. Methyl ammonium bromide and citric acid, prepare nanospherical carbon-coated lithium iron phosphate positive electrode material.

Benefits of technology

The compaction density and conductivity of lithium iron phosphate positive electrode material are significantly improved, the conductivity and stability of the material are enhanced, the energy density and rate performance are improved, and the problems of low electronic conductivity and slow lithium ion diffusion rate are solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954460A_ABST
    Figure CN118954460A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the compaction density of a lithium iron phosphate positive electrode material of a lithium ion battery, and relates to the technical field of compaction of lithium iron phosphate positive electrode materials of batteries. The method for improving the compaction density of the lithium iron phosphate positive electrode material of the lithium ion battery comprises the following specific steps; lithium carbonate and iron phosphate are placed in a drying chamber, and moisture and volatile organic compounds in the lithium carbonate and the iron phosphate are evaporated through high-temperature dry airflow; the lithium carbonate and the iron phosphate are compacted to obtain a powder material; after a carbon source is added, the mixture is put into a ball-milling tank to obtain a precursor; and preparing the nano spherical carbon-coated lithium iron phosphate through hydrothermal sintering. Corresponding metal ion doping and surface coating are carried out through iron phosphate, and the addition amount of citric acid is changed to control the morphological characteristics and particle size of the material, so that material agglomeration is reduced, and the positive electrode material with small particle size and uniform distribution is obtained by taking glucose as a carbon source, so that the compaction density of material arrangement is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of compaction of lithium iron phosphate positive electrode materials for batteries, and in particular to a method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries. Background Art

[0002] With the rapid development of the new energy vehicle industry, the power battery industry has grown rapidly, showing a strong demand growth. Lithium iron phosphate battery is the preferred lithium-ion battery for my country's new energy vehicles and large energy storage power stations. Lithium iron phosphate positive electrode material is an important component of lithium iron phosphate battery, which directly affects the energy density of the whole battery, high and low temperature adaptability, cycle attenuation, safety and stability and other important performance indicators.

[0003] Compared with ternary cathode materials, lithium iron phosphate has a low tap density and the compaction density of the prepared battery cell pole piece is low, which limits its energy density, causing the lithium iron phosphate industry to be suppressed by ternary cathode materials. However, lithium iron phosphate is an ideal material for lithium-ion battery cathode materials due to its low cost, better environmental protection, and high safety performance. In addition, the safety performance of passenger cars is gradually being paid attention to, and the market share of lithium iron phosphate is also increasing. If the problem of low compaction can be solved, the energy density of lithium iron phosphate cathode materials can be further improved.

[0004] At present, the mainstream methods for preparing lithium iron phosphate can be divided into three types according to the type of iron source: iron phosphate, ferrous oxalate and iron oxide. Among them, iron phosphate has a similar orthorhombic structure to lithium iron phosphate and has a small volume change. Using iron phosphate as the iron source and phosphorus source to prepare lithium iron phosphate can obtain better electrochemical performance. However, lithium iron phosphate has defects such as low electronic conductivity and low lithium ion diffusion coefficient, which hinders its industrial development. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium-ion batteries, which solves the problems raised in the above-mentioned background technology.

[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for improving the compaction density of lithium iron phosphate positive electrode material of lithium ion battery, comprising the following specific steps:

[0007] S1: Weigh lithium carbonate and iron phosphate according to the stoichiometric ratio, place the weighed lithium carbonate and iron phosphate in a drying chamber, and use high-temperature dry airflow to evaporate the moisture and volatile organic matter in them; the compaction density measured after the sample is dried will be significantly lower than the compaction density of the undried sample, and the repeatability and stability of the result will be better

[0008] The study found that under the action of external force, the mechanical interaction between powder particles will be enhanced, the gaps between particles will be filled, the atoms will have an attractive force and the contact area will increase, thus forming a powder tablet with a certain density and strength. Different pressures have different mechanical effects on powdered lithium iron phosphate, which in turn affects its compaction density results.

[0009] Without destroying the structure of the active material of the lithium iron phosphate powder material to be tested, the limit pressure it can withstand and the repeatability of its compaction density results under each pressure are tested. Within the safe pressure value range of the powder tablet press, when the pressure increases from 10MPa to 34MPa, the compaction density will gradually increase with the increase of pressure. For every 10MPa increase in pressure value, the compaction density will increase by about 0.2g / cm 3 .

[0010] In order to explore whether the length of the tableting time of lithium iron phosphate powder will have a corresponding impact on its compaction density results, the powder LiFePO4 samples of different masses were weighed and tableted under different pressures; the average height of the powder cake was measured after each tableting for a certain period of time, and its compaction density was calculated by the formula; the results showed that under no pressure, extending the tableting time of powder LiFePO4 will not greatly affect its compaction density results, and the pressure time will basically not affect the compaction density.

[0011] S2: The dried lithium carbonate and iron phosphate are placed in a powder tablet press, and the tablet press obtains powder material by compaction;

[0012] S3: After adding the carbon source to the powder material, put it into a ball mill, add an appropriate amount of anhydrous ethanol to make the ball-to-material mass ratio 3:1, and the solid content of the slurry is 40-50%. Mill it in a ball mill at a speed of 400-500r / min for 5-7h, and dry it at 80-90℃ to obtain a precursor;

[0013] S4: The ground precursor is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 500°C and kept for 5 hours, and then kept at 720°C for 10 hours. After sintering, a micro-nanostructured spherical carbon-coated lithium iron phosphate positive electrode material is prepared. Hexadecyltrimethylammonium bromide is added to the lithium iron phosphate positive electrode material as a cationic surfactant, and nano-spherical carbon-coated lithium iron phosphate is prepared by hydrothermal sintering.

[0014] The method uses iron phosphate as an iron source and a phosphorus source, lithium carbonate as a lithium source, and glucose, phenolic resin, ascorbic acid and starch as carbon sources to synthesize a carbon-coated lithium iron phosphate composite material.

[0015] The further improvement of the technical solution of the present invention is that: in addition to adding a carbon source to the powder material in S3, corresponding citric acid is added to control the particle size of FePO4·H2O, and the discharge specific capacity of lithium iron phosphate in S4 at a rate of 0.1C reaches 160mAH / g. The amount of citric acid added is changed to control the morphological characteristics and particle size of FePO4·H2O and reduce material agglomeration.

[0016] The further improvement of the technical solution of the present invention is that the carbon source in S3 is selected from glucose, phenolic resin, ascorbic acid and starch, and the lithium iron phosphate positive electrode material products obtained in S4 are all olivine-type lithium iron phosphate. Preferably, the particle size of olivine-type lithium iron phosphate is small and evenly distributed, so the compaction density is greater; using iron phosphate as the iron source and phosphorus source to prepare lithium iron phosphate can obtain better electrochemical performance, but lithium iron phosphate has defects such as low electronic conductivity and low lithium ion diffusion coefficient, which hinders its industrial development. The modification methods are roughly divided into three types: metal ion doping, nano-sizing and surface coating.

[0017] A further improvement of the technical solution of the present invention is that: the powder tablet press in S2 is pre-placed with 1% Cr 3+ , the precursor in S3 contains ferrous oxalate.

[0018] The further improvement of the technical solution of the present invention is that the secondary particle size of the carbon-coated lithium iron phosphate with micro-nano spherical structure after sintering in S4 is 1-2 μm, the primary particle size is less than 100 nm, the carbon content is 3%, and the tap density is 1.09 g / cm 3 , with a specific surface area of ​​22.49m 2 / g, and the 10C discharge specific capacity is 106.7mAh / g. Therefore, the nano-sized primary particles improve the material rate performance, and the micron-sized spherical secondary particles can obtain a high tap density while reducing agglomeration and maintaining the stability of the material.

[0019] Nano-sizing, high specific surface area and carbon coating can shorten the distance of lithium ion diffusion and electron migration, improve the conductivity of lithium iron phosphate positive electrode materials, and solve the problem of poor rate performance caused by low electronic conductivity and slow lithium ion diffusion rate.

[0020] A further improvement of the technical solution of the present invention is that the compaction pressure in S2 is gradually increased from 10 MPa to 40 MPa.

[0021] A further improvement of the technical solution of the present invention is that the hydrothermal temperature in S4 is 120° C. and the heating time is 5 hours.

[0022] A further improvement of the technical solution of the present invention is that the pre-drying treatment in S1 is performed at 60°C-120°C.

[0023] Beneficial Effects

[0024] The present invention provides a method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries. Compared with the prior art, it has the following beneficial effects:

[0025] The method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries controls the morphology and particle size of the material by doping and surface coating the iron phosphate with corresponding metal ions and adjusting the amount of citric acid added, thereby reducing material agglomeration, and using glucose as a carbon source to obtain a positive electrode material with a smaller particle size and uniform distribution, thereby improving the compaction density of the material, and the corresponding metal ion doping improves the conductivity of the material; and the overall material presents a micro-nano structure, forms a dense stack, reduces the carbon content in the material, obtains a positive electrode material with a high tap density, and improves the volumetric capacity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a flow chart of the specific steps of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides three technical solutions:

[0029] Embodiment 1:

[0030] A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries, comprising the following specific steps:

[0031] S1: Weigh lithium carbonate and iron phosphate according to the stoichiometric ratio, place the weighed lithium carbonate and iron phosphate in a drying chamber, and use high-temperature dry airflow to evaporate the moisture and volatile organic matter in them; the compaction density measured after the sample is dried will be significantly lower than the compaction density of the undried sample, and the repeatability and stability of the result will be better

[0032] The study found that under the action of external force, the mechanical interaction between powder particles will be enhanced, the gaps between particles will be filled, the atoms will have an attractive force and the contact area will increase, thus forming a powder tablet with a certain density and strength. Different pressures have different mechanical effects on powdered lithium iron phosphate, which in turn affects its compaction density results.

[0033] Without destroying the structure of the active material of the lithium iron phosphate powder material to be tested, the limit pressure it can withstand and the repeatability of its compaction density results under each pressure are tested. Within the safe pressure value range of the powder tablet press, when the pressure increases from 10MPa to 34MPa, the compaction density will gradually increase with the increase of pressure. For every 10MPa increase in pressure value, the compaction density will increase by about 0.2g / cm 3 .

[0034] In order to explore whether the length of the tableting time of lithium iron phosphate powder will have a corresponding impact on its compaction density results, the powder LiFePO4 samples of different masses were weighed and tableted under different pressures; the average height of the powder cake was measured after each tableting for a certain period of time, and its compaction density was calculated by the formula; the results showed that under no pressure, extending the tableting time of powder LiFePO4 will not greatly affect its compaction density results, and the pressure time will basically not affect the compaction density.

[0035] S2: The dried lithium carbonate and iron phosphate are placed in a powder tablet press, and the tablet press obtains powder material by compaction;

[0036] S3: After adding the carbon source to the powder material, put it into a ball mill, add an appropriate amount of anhydrous ethanol to make the ball-to-material mass ratio 3:1, and the solid content of the slurry is 40-50%. Mill it in a ball mill at a speed of 400-500r / min for 5-7h, and dry it at 80-90℃ to obtain a precursor;

[0037] S4: The ground precursor is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 500°C and kept for 5 hours, and then kept at 720°C for 10 hours. After sintering, a micro-nanostructured spherical carbon-coated lithium iron phosphate positive electrode material is prepared. Hexadecyltrimethylammonium bromide is added to the lithium iron phosphate positive electrode material as a cationic surfactant, and nano-spherical carbon-coated lithium iron phosphate is prepared by hydrothermal sintering.

[0038] The method uses iron phosphate as an iron source and a phosphorus source, lithium carbonate as a lithium source, and glucose, phenolic resin, ascorbic acid and starch as carbon sources to synthesize a carbon-coated lithium iron phosphate composite material.

[0039] Embodiment 2:

[0040] Based on Example 1:

[0041] In addition to adding a carbon source to the powder material in S3, corresponding citric acid is added to control the particle size of FePO4·H2O. The discharge specific capacity of S4 lithium iron phosphate at 0.1C rate reaches 160mAH / g. The amount of citric acid added is changed to control the morphology and particle size of FePO4·H2O and reduce material agglomeration.

[0042] The carbon source in S3 is selected from glucose, phenolic resin, ascorbic acid and starch, and the lithium iron phosphate positive electrode material products obtained in S4 are all olivine-type lithium iron phosphate. Preferably, the particle size of olivine-type lithium iron phosphate is small and evenly distributed, so the compaction density is greater; using iron phosphate as the iron source and phosphorus source to prepare lithium iron phosphate can obtain better electrochemical performance, but lithium iron phosphate has defects such as low electronic conductivity and low lithium ion diffusion coefficient, which hinders its industrial development. The modification methods are roughly divided into three types: metal ion doping, nano-ization and surface coating. This embodiment uses surface coating.

[0043] The powder tableting machine in S2 is pre-placed with Cr with a molar ratio of 1%. 3+ The precursor in S3 contains ferrous oxalate. In this embodiment, Cr 3+ Doping improves the conductivity of the material.

[0044] Embodiment three:

[0045] On the basis of Example 1 and Example 2: the carbon-coated lithium iron phosphate with micro-nano spherical structure after sintering in S4 has a secondary particle size of 1-2 μm, a primary particle size of less than 100 nm, a carbon content of 3%, and a tap density of 1.09 g / cm 3 , with a specific surface area of ​​22.49m 2 / g, and the 10C discharge specific capacity is 106.7mAh / g. Therefore, the nano-sized primary particles improve the material rate performance, and the micron-sized spherical secondary particles can obtain a high tap density while reducing agglomeration and maintaining the stability of the material.

[0046] Nano-sizing, high specific surface area and carbon coating can shorten the distance of lithium ion diffusion and electron migration, improve the conductivity of lithium iron phosphate positive electrode materials, and solve the problem of poor rate performance caused by low electronic conductivity and slow lithium ion diffusion rate.

[0047] The compaction pressure in S2 is gradually increased from 10 MPa to 40 MPa.

[0048] The hydrothermal temperature in S4 is 120° C. and the heating time is 5 h.

[0049] The pre-drying treatment in S1 is performed at 60°C-120°C.

[0050] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art, and the model parameters of each electrical appliance are not specifically limited, and conventional equipment can be used.

[0051] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium-ion batteries, It is characterized in that The specific steps include: S1: lithium carbonate and iron phosphate are weighed according to a stoichiometric ratio, and the weighed lithium carbonate and iron phosphate are placed in a drying chamber, and water and volatile organic matter therein are evaporated by using a high-temperature dry air flow; S2: The dried lithium carbonate and iron phosphate are placed in a powder tablet press, and the tablet press obtains powder material by compaction; S3: After adding the carbon source to the powder material, put it into a ball mill, add an appropriate amount of anhydrous ethanol to make the ball-to-material mass ratio 3:1, and the solid content of the slurry is 40-50%. Mill it in a ball mill at a speed of 400-500r / min for 5-7h, and dry it at 80-90℃ to obtain a precursor; S4: The ground precursor is placed in a tubular furnace, and in a nitrogen atmosphere, the temperature is raised to 500°C and kept for 5 hours, and then kept at 720°C for 10 hours. After sintering, a micro-nanostructured spherical carbon-coated lithium iron phosphate positive electrode material is prepared. Hexadecyltrimethylammonium bromide is added to the lithium iron phosphate positive electrode material as a cationic surfactant, and nano-spherical carbon-coated lithium iron phosphate is prepared by hydrothermal sintering.

2. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: In the S3, in addition to adding a carbon source, corresponding citric acid is added to control the FePO 4 ·H 2 O particle size, the S4 lithium iron phosphate has a discharge specific capacity of 160mAH / g at a rate of 0.1C.

3. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The carbon sources in S3 are glucose, phenolic resin, ascorbic acid and starch, and the lithium iron phosphate positive electrode material products obtained in S4 are all olivine-type lithium iron phosphate.

4. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The powder tableting machine in S2 is pre-placed with Cr with a molar ratio of 1%. 3+ , the precursor in S3 contains ferrous oxalate.

5. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The carbon-coated lithium iron phosphate with a micro-nano spherical structure after sintering in S4 has a secondary particle size of 1-2 μm, a primary particle size of less than 100 nm, a carbon content of 3%, and a tap density of 1.09 g / cm 3 , with a specific surface area of ​​22.49m 2 / g, and the 10C discharge specific capacity is 106.7mAh / g.

6. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The compaction pressure in S2 is gradually increased from 10 MPa to 40 MPa.

7. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The hydrothermal temperature in S4 is 120° C. and the heating time is 5 h.

8. A method for improving the compaction density of lithium iron phosphate positive electrode materials for lithium ion batteries according to claim 1, Features: The pre-drying treatment in S1 is performed at 60°C-120°C.

Citation Information

Patent Citations

  • Method for preparing carbon-coated lithium iron phosphate positive-pole material

    CN108110238A

  • Lithium iron phosphate-based composite material with capacity higher than theoretical capacity of lithium iron phosphate, preparation method and use of lithium iron phosphate-based composite material

    CN108735997A

  • Grid-structured carbon-coated lithium iron phosphate nanoparticles and preparation method and application thereof

    CN112794301A

  • Organic carbon coated lithium iron phosphate positive electrode material and preparation method thereof

    CN113651304A