Battery
By controlling the particle size distribution and element content of the positive and negative electrode active materials in lithium batteries, combined with carbon-based materials, the problem of side effects of materials is solved, and the battery performance with high energy density and cycle stability is achieved.
Patent Information
- Application Number
- CN202411108478.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing lithium batteries have material side effects in improving energy density and cycle stability, such as irreversible phase change of the positive electrode material and expansion and extension of the negative electrode material, resulting in a degradation of battery performance.
By controlling the particle size distribution and element content in the positive electrode and negative electrode active materials, a specific relationship is met to improve the surface density and compaction density of the positive electrode sheet, alleviate side reactions and expansion problems, and at the same time, add carbon-based to the negative electrode active materials. Material to reduce volume expansion.
The high energy density and good cycle stability of the battery are achieved, the rate charging performance and electrochemical performance are improved, and the excessive extension of the pole sheet and the problem of belt breakage are avoided.
Smart Images

Figure CN119008939A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a battery. Background Art
[0002] Lithium-ion batteries bring convenience to people. At the same time, in order to meet people's growing needs, the technology of lithium batteries is also developing rapidly, and the main development direction is to improve performance and ensure safety. The main performance of lithium batteries is rate charging and higher energy density. How to select various materials and cooperate with each other to make them play the best performance is also an indispensable research content. However, one battery system often cannot take into account all battery performance. Therefore, for specific needs, a battery system can be designed in a targeted manner to achieve the goal.
[0003] In order to improve the energy density of the battery, the material can be improved by increasing the gram capacity of the active material, such as using lithium cobalt oxide materials with high cut-off voltage for the positive electrode and silicon-based materials for the negative electrode. The core structure can be improved by increasing the surface density and compaction density. However, these methods will bring some side effects. High cut-off voltage may cause irreversible phase change of the material, causing the battery capacity to decay, while silicon-based materials may cause the negative electrode to expand and extend. In order to overcome the side effects of the material and demonstrate its superior performance, it is necessary to design the structural system of the battery and reduce the impact between various materials through overall matching. Summary of the invention
[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and to provide a battery having high energy density and good cycle stability and electrochemical performance.
[0005] In order to achieve the above-mentioned object, the present invention provides a battery, the battery comprising a positive electrode sheet and a negative electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising an aluminum element, and the volume particle size of the positive electrode active material presents a bimodal distribution, the positive electrode active material layer comprises a positive electrode active material containing an Al element, the volume particle size of the positive electrode active material presents a bimodal distribution, and the particle sizes corresponding to the two peaks are F1 and F2, respectively, in units of μm; F1<F2; the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer arranged on the surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material, and the negative electrode active material comprises a silicon-based material and a carbon-based material;
[0006] The battery satisfies the relationship: K1 = (Ac / 400-1000 / (5*F1+2*F2)+(σ-
[0007] (Ws+1)*(F3+50) / 2)≥407;
[0008] Wherein, Ac is the mass content of aluminum element in the positive electrode active material, in ppm;
[0009] Ws is the mass content of silicon in the negative electrode active material;
[0010] F3 is the particle size corresponding to the highest peak in the volume particle size distribution curve of the negative electrode active material, in μm;
[0011] σ is the fracture strength of the negative electrode current collector, in MPa.
[0012] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0013] The present invention can increase the surface density and compaction density of the positive electrode sheet, stabilize the structure of the positive electrode active material, reduce the side reaction between the positive electrode active material and the electrolyte, alleviate the gas production and active lithium consumption of the battery, and improve the cycle stability of the battery by controlling the particle size of the negative electrode active material, the silicon content and the fracture strength of the negative electrode current collector to meet the above relationship. The volume expansion caused by the silicon-based material can be alleviated, and then the problems of gas production and lithium precipitation caused by the expansion can be alleviated. It can also improve the yield of the battery core, avoid the problems of excessive extension of the pole piece and the broken band of the pole piece that may occur during the cycle, and improve the rate charging performance and cycle performance of the battery. By controlling the particle size of the positive electrode active material containing two particle sizes, the highest peak particle size of the negative electrode active material, the addition amount of Al element in the positive electrode active material and silicon element in the negative electrode active material, and the fracture strength of the negative electrode current collector, the battery has a high energy density, and at the same time has good cycle stability and electrochemical performance.
[0014] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the volume particle size distribution diagram of the positive electrode active material in Example 1. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0017] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0018] The present invention provides a battery, the battery comprising a positive electrode sheet and a negative electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising an aluminum element, and the volume particle size of the positive electrode active material presents a bimodal distribution, the positive electrode active material layer comprising a positive electrode active material containing an Al element, the volume particle size of the positive electrode active material presents a bimodal distribution, and the particle sizes corresponding to the two peaks are F1 and F2, respectively, in units of μm; F1<F2; the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer arranged on the surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material, and the negative electrode active material comprises a silicon-based material and a carbon-based material;
[0019] The battery satisfies the relationship: K1 = (Ac / 400-1000 / (5*F1+2*F2)+(σ-
[0020] (Ws+1)*(F3+50) / 2)≥407 (its value can be 407, 420, 440, 460, 480, 500, 520, 540, 560, 580, 600);
[0021] Wherein, Ac is the mass content of aluminum element in the positive electrode active material, in ppm;
[0022] Ws is the mass content of silicon in the negative electrode active material;
[0023] F3 is the particle size corresponding to the highest peak in the volume particle size distribution curve of the negative electrode active material, in μm;
[0024] σ is the fracture strength of the negative electrode current collector, in MPa.
[0025] The particle size distribution of the positive electrode active material has two peaks, large and small, reflecting that the positive electrode active material is composed of particle gradations of two sizes. When the matching method satisfies the relationship, the compactness of the positive electrode active material particles can be improved, the surface density and compaction density of the positive electrode sheet can be improved, and the positive electrode sheet can load more active materials in a limited space, thereby providing more energy for the battery. At the same time, the matching of large and small particle sizes also improves the performance of the positive electrode sheet, such as improving the processing performance of the electrode sheet, improving the bonding performance between the particles and the glue, improving the flexibility of the electrode sheet, and improving the rate performance of the positive electrode sheet. Doping with Al elements has a great influence on the performance of the positive electrode active material. Doping with positive electrode active materials that meet the relationship can increase the cutoff voltage of the positive electrode active material, improve the high temperature stability of the positive electrode active material, ensure that the positive electrode has a larger gram capacity, and can also meet the capacity retention of the high temperature cycle of the battery cell. Adding silicon-based materials to the negative electrode active material can further increase the gram capacity of the negative electrode, reduce the coating surface density of the negative electrode, and reduce the space occupied by the negative electrode sheet, thereby improving the energy density of the battery. The content of silicon material can affect the expansion and extension of the negative electrode sheet. During the charge and discharge process, the repeated expansion and recovery of silicon particles in the negative electrode sheet can easily lead to relative displacement between particles and between particles and current collectors, which ultimately leads to increased surface resistance of the electrode sheet, powder loss, and increased expansion and extension of the electrode sheet, increasing the squeeze on the membrane shell, and ultimately causing battery failure. The current collector and negative electrode active material that satisfy the relationship in the relationship can effectively alleviate the stress effect of silicon material expansion on the electrode sheet, reduce the expansion and extension of the electrode sheet, and enjoy the high gram capacity provided by silicon materials while preventing the expansion and extension of the electrode sheet caused by silicon particles.
[0026] In some embodiments, Ac is 5000-9000, such as 5000, 5500, 6000, 6500, 7000, 7500, 8000, 8500, 9000. The type and content of doping elements in the positive electrode active material will have a great impact on its performance. The presence of Al element increases the working voltage of the positive electrode active material, thereby increasing the gram capacity of the positive electrode active material. At the same time, the Al-O bond is more stable, which plays a stabilizing role in the structure of the positive electrode active material, and can also inhibit the dissolution of cobalt, thereby enhancing the high temperature and cycle stability of the positive electrode active material. Too little Al doping results in failure to satisfy the relationship, which will lead to poor cycle stability; too much Al doping reduces the gram capacity of the positive electrode active material, thereby reducing the battery energy density.
[0027] In the present invention, the content of elements can be obtained by ICP testing.
[0028] In some embodiments, F1 is 2-8, such as 2, 3, 4, 5, 6, 7, 8. In some embodiments, F2 is 12-25, such as 12, 14, 16, 18, 20, 22, 25. The volume particle size of the positive electrode active material is bimodal and satisfies the relationship, so that small particles can fill the gaps between large particles, which can increase the surface density of the positive electrode sheet, facilitate the rolling of the positive electrode sheet and increase the compaction density, thereby increasing the energy density of the battery cell and reducing the thickness rebound of the electrode sheet; it can also increase the contact area between the positive electrode surface and the electrolyte, increase the contact area between the positive electrode active material particles, increase the speed of ion transfer, and prevent the excessive surface area of the particles and the increase of the electrolyte side reaction, resulting in gas production and active lithium consumption. When F1 is too large or F2 is too small, it will lead to problems such as too small compaction density of the electrode sheet, thicker electrode sheet, and reduced flexibility of the electrode sheet, which affect the energy density and process yield. If F1 is too small or F2 is too large, it will lead to problems such as increased battery side reactions or reduced rate performance.
[0029] In the present invention, the particle size of the material can be measured by a laser particle size analyzer.
[0030] In some embodiments, the positive electrode sheet satisfies: 0.38*Yc<(F2-5) / F1<0.4*Mc; wherein Yc is the compaction density of the positive electrode sheet, in g / cm 3 ; Mc is the surface density of the positive electrode active material layer, in mg / cm 2 .
[0031] In some embodiments, Yc is 3-5, such as 3, 3.5, 4, 4.5, or 5.
[0032] In some embodiments, Mc is 11.2-19.8, such as 11.2, 12, 13, 14, 15, 16, 17, 18, 19, 19.8.
[0033] In the present invention, the surface density of the pole piece can be cut as follows: 15.0425 cm 2 Weigh the disc, subtract the weight of the foil, and divide the weight by the area to calculate the surface density. The compacted density can be calculated by dividing the surface density by the thickness of the coating.
[0034] In some embodiments, the positive electrode active material comprises at least one of the following substances doped with aluminum or undoped with aluminum: lithium nickel cobalt manganese oxide, lithium nickel cobalt oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, preferably comprising lithium cobalt oxide doped with aluminum or undoped with aluminum and / or lithium nickel cobalt manganese oxide doped with aluminum or undoped with aluminum.
[0035] In some embodiments, the positive electrode active material layer further comprises a conductive agent and a binder. The conductive agent and the binder may be conventional conductive agents and binders in the art. In one embodiment, the conductive agent includes but is not limited to at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber. In one embodiment, the binder includes but is not limited to at least one of carboxymethyl cellulose CMC (or its sodium salt), polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyethylene oxide, and polyvinylidene fluoride.
[0036] In some embodiments, in the positive electrode active material layer, the content of the positive electrode active material is 94wt% to 98.5wt%, such as 94wt%, 95wt%, 96wt%, 97wt%, 98wt%, and 98.5wt%; the content of the binder is 0.7wt% to 5wt%, such as 0.7wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, and 5wt%; the content of the conductive agent is 0.8wt% to 5wt%, such as 0.8wt%, 1wt%, 2wt%, 3wt%, 4wt%, and 5wt%.
[0037] In some embodiments, the positive electrode current collector may be aluminum foil or composite aluminum foil.
[0038] In some embodiments, F3 is 6-20, such as 6, 8, 10, 12, 14, 16, 18, 20. The particle size of the negative electrode active material will affect the compaction density of the negative electrode sheet and the thickness rebound of the electrode sheet. When F3 is small, the gap between the particles is small, and the space for expansion is smaller. At the same time, the thickness rebound of the electrode sheet after rolling is large, which can easily lead to poor thickness of the battery cell manufacturing and excessive cycle expansion. When F3 is large, it will affect the rate performance of the battery cell, increase the distance of lithium ion embedding, increase the polarization internal resistance of the battery, etc. If the relationship range is not satisfied due to the size of F3, the expansion of the negative electrode sheet will increase and the process defect rate caused by the thickness of the winding core will increase, and the rate charging performance and cycle performance of the battery will be affected.
[0039] In the present invention, a laser diffraction particle size analyzer is used for measurement.
[0040] In some embodiments, Ws is 1%-20%, such as 1%, 5%, 10%, 15%, and 20%. Adding silicon to the negative electrode sheet can effectively increase the gram capacity of the negative electrode, thereby reducing the surface density of the negative electrode sheet, reducing the amount of negative electrode active material, and increasing the energy density of the battery. However, the presence of silicon can cause a series of problems such as expansion and extension of the negative electrode sheet and volume expansion, gas production, and lithium precipitation of the battery, thereby reducing the cycle life of the battery. Using a silicon content and a material particle size that satisfy the range in the relationship, combined with a negative electrode current collector of suitable strength, combined with a positive electrode sheet, can not only give play to the advantages of high energy density and good material stability of the positive and negative electrode sheets, but also avoid the risk of cycle failure caused by expansion and extension of the electrode sheet, alleviate problems such as volume expansion, gas production, and lithium precipitation, and make the battery have excellent cycle performance and rate charging performance.
[0041] In the present invention, the test method of Ws can be: negative electrode ash test, weigh more than 2g of negative electrode active material, record the weight W1, keep it warm in 800℃ air for 10 hours, cool it to room temperature, and record the weight W2, Ws=W2 / W1.
[0042] In some embodiments, σ≥400, for example, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, preferably, σ≥500. The strength of the negative electrode current collector affects the yield of the manufacturing process of the core, as well as the occurrence of problems such as excessive extension of the pole piece and pole piece breakage that may occur during the battery cycle. In some embodiments, the negative electrode current collector may be a copper foil or a composite current collector.
[0043] In the present invention, the fracture strength of the negative electrode current collector can be tested as follows: the current collector (foil) is cut into strips of 15 mm ± 0.2 mm, and the two ends of the foil are clamped in the clamps using a WD-D3 electronic universal testing machine with a gap of 50 mm between the upper and lower clamps, and the test is started at a speed of 100 mm / min until the equipment stops testing, and the fracture strength σ is recorded. The error of the test is no more than 10% for 3 times, and the average value is taken.
[0044] In some embodiments, the negative electrode active material layer further comprises a conductive agent. The type of the conductive agent can refer to the type in the positive electrode active material layer, and can be the same or different when used.
[0045] In some embodiments, the negative electrode sheet satisfies: 86<Ma+2*Ya+80*Wa<90, for example, it can be 86.1, 96.5, 87, 87.5, 88, 88.5, 89, 89.5, 89.9; wherein Ya is the compaction density of the negative electrode sheet, in g / cm 3 ; Ma is the density of the negative electrode active material layer, in mg / cm 2; Wa is the total mass content of the negative electrode active material and the conductive agent in the negative electrode active material layer.
[0046] In some embodiments, Ya is 0.9-1.9, such as 0.9, 1, 1.2, 1.4, 1.6, 1.8, or 1.9.
[0047] In some embodiments, Ma is 4-12, such as 4, 6, 8, 10, or 12.
[0048] In some embodiments, Wa is 96%-99%, such as 96%, 97%, 98%, or 99%.
[0049] In the present invention, the test method of Wa can be tested using a thermogravimetric analyzer, the sample is kept at 80°C for 2h, 0.05g of the sample is placed in an alumina crucible, and heated to 600°C at 10°C / min in a nitrogen environment, and the residual weight is Wa.
[0050] In some embodiments, the carbon-based material comprises at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, and soft carbon.
[0051] In some embodiments, the silicon-based material includes a silicon-carbon material, a silicon-oxygen material (SiO x , x<2) and at least one of nano silicon materials.
[0052] In some embodiments, the negative electrode active material comprises artificial graphite and silicon carbon material.
[0053] In some embodiments, the negative electrode active material layer further comprises a binder. The type of the binder can refer to the type of the positive electrode active material layer, and can be the same or different when used.
[0054] In some embodiments, in the negative electrode active material layer, the content of negative electrode active material is 95wt% to 99wt%, for example, 95wt%, 96wt%, 97wt%, 98wt%, and 99wt%, the content of binder is 0.5wt% to 3wt%, for example, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, and 3wt%, and the content of conductive agent is 0.5wt% to 2wt%, for example, 0.5wt%, 1wt%, 1.5wt%, and 2wt%.
[0055] In some embodiments, the battery is a lithium-ion battery.
[0056] In some embodiments, the battery further comprises a separator and an electrolyte, and the positive electrode sheet, the separator and the negative electrode sheet are stacked.
[0057] In some embodiments, the diaphragm comprises a base film. The base film can be made of conventional materials in the art, including but not limited to at least one of polyethylene, polypropylene, glass fiber, and non-woven fabric. The diaphragm can be a single-layer film or a multi-layer composite film.
[0058] In some embodiments, the battery comprises a battery assembly and a shell in which a positive electrode sheet, a separator and a negative electrode sheet are stacked, and the battery assembly is located in the shell. The shell may be an aluminum-plastic film. The battery may be a soft-pack battery.
[0059] In some embodiments, the electrolyte comprises an organic solvent and a lithium salt.
[0060] In some embodiments, the organic solvent comprises carbonate and / or carboxylate.
[0061] In some embodiments, the organic solvent comprises at least one of the following fluorinated or unsubstituted solvents: propyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, methyl propionate, propyl propionate (PP), ethyl propionate (EP), methyl butyrate, ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate, diethyl carbonate (DEC), and ethyl methyl carbonate.
[0062] In some embodiments, the lithium salt comprises at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium bisfluorosulfonyl imide (LiTFSI), lithium bistrifluoromethylsulfonyl imide, lithium difluorobisoxalatophosphate, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium, and lithium bis(trifluoromethylsulfonyl)imide.
[0063] In some embodiments, the concentration of lithium salt in the electrolyte is 0.8 mol / L-2 mol / L, for example, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, or 2 mol / L.
[0064] In some embodiments, the electrolyte further comprises a functional additive.
[0065] In some embodiments, the functional additives include one or more of nitrile additives, carbonate additives, and organic sulfur additives.
[0066] In some embodiments, the nitrile additive includes at least one of ethylene glycol bis(propionitrile) ether, adiponitrile, succinonitrile (SN), 1,3,6-hexanetrinitrile (HTCN), glutaronitrile, trans-butenedinitrile, and trans-hexenedinitrile.
[0067] In some embodiments, the carbonate additive includes at least one of fluoroethylene carbonate (FEC), bisfluoroethylene carbonate, vinylene carbonate (VC), and vinyl ethylene carbonate (VEC).
[0068] In some embodiments, the organic sulfur additive comprises at least one of 1,3-propane sultone (PS), 1,3-propylene sultone, 2,4-butane sultone, 1,4-butane sultone, and methylene methane disulfonate.
[0069] In some embodiments, the content of each component in the electrolyte can be a conventional amount in the art, which will not be described in detail herein. The electrolyte can be commercially available.
[0070] If there is no special explanation, other options of the lithium battery are conventional options in the art. The battery can be assembled in a conventional manner in the art.
[0071] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0072] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0073] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0074] The method for determining the parameters of the positive and negative electrodes in the battery in the embodiment includes:
[0075] (1) Fracture strength of negative electrode sheet: Cut the copper foil into small strips of 15 mm ± 0.2 mm, use WD-D3 electronic universal testing machine, with a gap of 50 mm between the upper and lower clamps, clamp the two ends of the foil in the clamps respectively, start the test at a speed of 100 mm / min, until the equipment stops testing, and record the fracture strength σ. The error of the test is no more than 10% for 3 times, and the average value is taken.
[0076] (2) Aluminum content in the positive electrode: tested using ICP.
[0077] (3) Particle size distribution test of the positive electrode active material in the positive electrode sheet: measured using a laser diffraction particle size analyzer.
[0078] (4) Pole surface density: cut 15.0425cm 2Weigh the disc, subtract the weight of the foil, and divide the weight by the area to calculate the surface density.
[0079] (5) Compacted density of the electrode: the surface density divided by the thickness of the active material layer.
[0080] (6) Testing method of Ws: For the negative electrode sheet ash content test, weigh more than 2 g of negative electrode active material and record the weight W1. Keep it in air at 800°C for 10 hours. After cooling to room temperature, record the weight W2. Ws = W2 / W1.
[0081] (7) Wa test method: Use a thermogravimetric analyzer to test. Keep the sample at 80°C for 2 h. Take 0.05 g of the sample and put it in an alumina crucible. Heat it to 600°C at 10°C / min in a nitrogen environment. The remaining weight is Wa.
[0082] Example 1 Group
[0083] This example is used to illustrate the method for preparing the battery of the present invention.
[0084] In Examples 1-1 to 1-4, copper foils with different fracture strengths σ were used as negative electrode current collectors, and the specific preparation method of the battery was as follows.
[0085] Positive electrode sheet: The positive electrode active material (two kinds of lithium cobalt oxide with different particle sizes, the particle size distribution diagram is as follows Figure 1 As shown in FIG. 1 ), conductive carbon black, carbon nanotubes, and PVDF are stirred into slurry in NMP at a weight ratio of 95:1:1.5:2.5, and then coated on aluminum foil, dried, rolled, cut, welded to the electrode ears, and pasted with adhesive tape to prepare a positive electrode sheet. The lithium cobalt oxide is doped with aluminum.
[0086] Negative electrode sheet: CMC is added to deionized water, and then graphite, silicon carbon particles, conductive carbon black and carbon nanotubes are added and stirred into slurry, and finally PAA and SBR are added and stirred to obtain slurry (the weight ratio of graphite, silicon carbon material, conductive carbon black, carbon nanotubes, CMC, PAA, and SBR is 88:10:0.1:0.1:0.3:1:0.5, that is, Wa is 98.20%), and the slurry is coated on the negative electrode collector, and then baked, rolled, cut, welded to the pole ear, and taped to prepare the negative electrode sheet. The compacted density Ya of the negative electrode sheet is 1.62g / cm 3 ; The negative electrode active material layer density Ma is 6.33 mg / cm 2 . K3=Ma+2*Ya+80*Wa=88.13.
[0087] Electrolyte: Ethylene carbonate (EC), fluoroethylene carbonate (FEC), and diethyl carbonate (DEC) were prepared as an organic solvent in a weight ratio of 2.5:0.5:7, and then lithium hexafluorophosphate was added thereto at a final concentration of 1 mol / L.
[0088] Diaphragm: Use PE base film.
[0089] The positive and negative electrodes are separated by a separator, wound into a core, and then encapsulated in an aluminum-plastic film shell. After baking, liquid injection, formation, and secondary sealing, the battery is prepared.
[0090] The volume particle size of the positive electrode active material is bimodal, and the particle sizes corresponding to the two peaks are F1 and F2, respectively, in μm; F1<F2; Ac is the mass content of aluminum in the positive electrode active material, in ppm; Ws is the mass content of silicon in the negative electrode active material; F3 is the particle size corresponding to the highest peak in the volume particle size distribution curve of the negative electrode active material, in μm; σ is the fracture strength of the negative electrode current collector, in MPa; K1=(Ac / 400-1000 / (5*F1+2*F2)+(σ-(Ws+1)*(F3+50) / 2); K2=(F2-5) / F1; Yc is the compaction density of the positive electrode sheet, in g / cm 3 ; Mc is the surface density of the positive electrode active material layer, in mg / cm 2 , the specific values are shown in Table 1.
[0091] Comparative Example 1
[0092] The operation was carried out according to the method described in Example 1-1, except that the fracture strength σ of the negative electrode current collector was different, as shown in Table 1.
[0093] Example 2 and Comparative Example 2
[0094] The operation was carried out according to the method described in Example 1-1, except that the content of aluminum element doped in the lithium cobalt oxide was different, as shown in Table 1.
[0095] Example 3 and Comparative Example 3
[0096] The operation was carried out according to the method described in Example 1-1, except that F1 was different, as shown in Table 1.
[0097] After calculation, the prepared positive electrode sheets all satisfy 0.38*Yc<(F2-5) / F1<0.4*Mc.
[0098] Example 4 and Comparative Example 4
[0099] The operation was carried out according to the method described in Example 1-1, except that F2 was different, as shown in Table 1.
[0100] After calculation, the prepared positive electrode sheets all satisfy 0.38*Yc<(F2-5) / F1<0.4*Mc.
[0101] Example 5 and Comparative Example 5
[0102] The operation was carried out according to the method described in Example 1-1, except that the mass content Ws of silicon element in the negative electrode active material was different, as shown in Table 1.
[0103] Example 6 and Comparative Example 6
[0104] The operation was carried out according to the method described in Example 1-1, except that F3 was different, as shown in Table 1.
[0105] Example 7
[0106] The operation was carried out according to the method described in Example 1-1, except that Wa was different, 94%, and Ya and Ma were kept unchanged, K3 = Ma + 2*Ya + 80*Wa = 84.77.
[0107] Table 1
[0108]
[0109]
[0110] Note: In Table 1, “*” indicates the same as Example 1-1.
[0111] Test Case
[0112] The performance of the batteries prepared in the examples and comparative examples is tested below, and the specific operations are as follows.
[0113] (1) Negative electrode elongation test: The battery was cycled at a constant temperature of 25°C, charged at a constant current of 1C to 4.5V, charged at a constant voltage of 4.5V to 0.2C, and discharged at 0.7C to 3V. After 500 cycles of the cycle test, the battery was discharged to 3V, the battery was dissected, and the width of the electrode was tested using a 2.5D microscopy tester. The width of the electrode farthest from the active material layer in the double-sided empty foil area was recorded as S1, and the width of the active material layer area of the electrode was recorded as S2. The elongation of the electrode was (S2-S1) / S1. The average value of the five values was taken.
[0114] (2) Battery energy density: Use the Xinwei battery tester to charge at 0.2C to the upper voltage limit (cutoff 0.02C) / discharge at 0.2C to the lower voltage limit, repeat 3 times, and take the third discharge energy as the battery cell energy Q. Use a 2.5D microscope tester to test the width W and height H of the battery cell, and use a PPG thickness tester to test the full-charge thickness L of the battery cell, then the energy density is Q / (W*H*L).
[0115] (3) Battery room temperature cycle performance test: At 25°C, charge at 1C to the cut-off voltage, charge at constant voltage to the cut-off current of 0.05C, and discharge at 1C to the lower limit voltage. Repeat the above charge and discharge steps 800 times.
[0116] Calculation method of expansion rate after 50 cycles: fully charge the battery, test the full-charge thickness H1, cycle 50T according to the cycle system, fully charge the battery, test the thickness after the cycle H2, cycle expansion rate = (H2-H1) / H1*100%.
[0117] Capacity retention rate after 200 cycles: The capacity of the battery after one cycle is recorded as R1, and the capacity after 200 cycles is recorded as R2. Capacity retention rate = R2 / R1*100%.
[0118] (4) Battery high temperature cycle performance test: The battery was kept at a constant temperature of 45°C for 1 h, then charged at 1C to the cut-off voltage, charged at a constant voltage to a cut-off current of 0.05C, and discharged at 1C to the lower limit voltage. The above charge and discharge steps were repeated 800 times.
[0119] Calculation method of expansion rate after 50 cycles: fully charge the battery, test the full-charge thickness H1, cycle 50T according to the cycle system, fully charge the battery, test the thickness after the cycle H2, cycle expansion rate = (H2-H1) / H1*100%.
[0120] Capacity retention rate after 200 cycles: The capacity of the battery after one cycle is recorded as R1, and the capacity after 200 cycles is recorded as R2. Capacity retention rate = R2 / R1*100%.
[0121] (5) 25℃ rate charging performance test
[0122] Calculation method of constant current charging ratio for 25℃ rate charging: 1. Constant current discharge, 0.5C discharge cut-off voltage is 3V; 2. Constant current charging, 1.5C charging, cut-off voltage is 4.5V, the charging capacity of this step is recorded as R3; 3. Constant voltage charging, cut-off current is 0.05C, the charging capacity of this step is recorded as R4; constant current charging ratio = R3 / (R3+R4).
[0123] The results of the above tests are shown in Table 2.
[0124] Table 2
[0125]
[0126] It should be noted that, in this article, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the method and device in the embodiment of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A battery, It is characterized in that The battery comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, wherein the positive electrode active material comprises an aluminum element, and the volume particle size of the positive electrode active material presents a bimodal distribution, and the particle sizes corresponding to the two peaks are F and F, respectively. 1 and F 2 , unit is μm; F 1 <F 2 The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a silicon-based material and a carbon-based material; The battery satisfies the relationship: K 1 =(Ac / 400-1000 / (5*F 1 +2*F 2 )+(σ- (Ws+1)*(F 3 +50) / 2)≥407; Wherein, Ac is the mass content of aluminum element in the positive electrode active material, in ppm; Ws is the mass content of silicon in the negative electrode active material; F 3 is the particle size corresponding to the highest peak in the volume particle size distribution curve of the negative electrode active material, in μm; σ is the fracture strength of the negative electrode current collector, in MPa.
2. The battery according to claim 1, It is characterized in that Ac is 5000-9000; and / or F 1 is 2-8; and / or F 2 is 12-25; and / or F 3 is 6-20; and / or Ws is 1%-20%; and / or σ≥400, preferably, σ≥500.
3. The battery according to claim 1 or 2, It is characterized in that The positive electrode sheet satisfies: 0.38*Yc<(F 2 -5) / F 1 <0.4*Mc; Among them, Yc is the compaction density of the positive electrode sheet, in g / cm 3 ; Mc is the surface density of the positive electrode active material layer, in mg / cm 2 .
4. The battery according to claim 3, It is characterized in that Yc is 3-5; and / or Mc is 11.2-19.
8.
5. The battery according to any one of claims 1 to 4, It is characterized in that The positive electrode active material contains at least one of the following substances doped with aluminum or undoped with aluminum: lithium nickel cobalt manganese oxide, lithium nickel cobalt oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, preferably lithium cobalt oxide doped with aluminum or undoped with aluminum and / or lithium nickel cobalt manganese oxide doped with aluminum or undoped with aluminum.
6. The battery according to any one of claims 1 to 5, It is characterized in that The negative electrode active material layer further comprises a conductive agent; Preferably, the negative electrode sheet satisfies: 86<Ma+2*Ya+80*Wa<90; Among them, Ya is the compaction density of the negative electrode sheet, in g / cm 3 ; Ma is the density of the negative electrode active material layer, in mg / cm 2 ; Wa is the total mass content of the negative electrode active material and the conductive agent in the negative electrode active material layer.
7. The battery according to claim 6, It is characterized in that Ya is 0.9-1.9; and / or Ma is 4-12; and / or Wa is 96%-99%.
8. The battery according to any one of claims 1 to 7, It is characterized in that The carbon-based material comprises at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon and soft carbon; and / or The silicon-based material comprises at least one of silicon-carbon particles, silicon-oxygen particles and nano-silicon particles; Preferably, the negative electrode active material comprises artificial graphite and silicon carbon particles.
9. The battery according to any one of claims 1 to 8, It is characterized in that The battery is a lithium-ion battery.
10. The battery according to any one of claims 1 to 9, It is characterized in that The battery also comprises a separator and an electrolyte, and the positive electrode sheet, the separator and the negative electrode sheet are stacked.
Citation Information
Patent Citations
Positive plate and battery
CN118198262A
Negative active material, negative plate and battery
CN118431448A
Positive electrode and lithium secondary battery comprising same
WO2024136465A1
Cited By
Negative pole piece, secondary battery and electric device
CN119786527A
Secondary battery and electric device
CN120048855A