Alpha aluminum oxide and preparation method thereof
By pretreatment and high-temperature calcination of industrial alumina, combined with CO2 introduction and boric acid, the problem of calcined α alumina being difficult to take into account ultra-low sodium and spherical phases, and high-quality spherical α alumina is achieved Preparation meets the high-quality requirements of industrial ceramics.
Patent Information
- Application Number
- CN202411366574.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing technology is difficult to take into account both the ultra-low sodium and spherical phases of calcined α alumina, which affects its quality requirements in the wear-resistant ceramics, ceramic glaze and other industries.
By pretreating industrial alumina to remove impurities and reduce sodium content, then mixing with mineralizers and calcining under high temperature conditions, ensuring spherical conversion of α alumina, using CO2 inlet and boric acid as mineralizer to promote crystallization Grain growth and morphology adjustment.
The preparation of spherical α alumina with a sodium oxide content of less than 0.02% and a grain size of 1.8μm to 2.2μm was achieved, which improved the calcination quality and morphological consistency and met the high-quality requirements of industrial ceramics.
Smart Images

Figure CN118954560A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of aluminum oxide preparation, and in particular to alpha aluminum oxide and a preparation method thereof. Background Art
[0002] As raw materials for industrial ceramics, calcined α alumina series products are widely used in wear-resistant ceramics, ceramic glazes, refractory materials and other industries. Especially as the quality requirements of industrial ceramics are gradually improved, users have higher requirements on the quality of calcined α alumina.
[0003] However, there is currently a defect that it is difficult to simultaneously take into account the ultra-low sodium and spherical phase of calcined α-alumina. Summary of the invention
[0004] The present application provides an alpha alumina and a preparation method thereof to solve the following technical problem: how to reduce the sodium content of spherical alpha alumina.
[0005] In a first aspect, the present application provides a method for preparing alpha alumina, the method comprising:
[0006] Pre-treating industrial alumina to obtain alumina with a target sodium oxide content;
[0007] Mixing the alumina having a target sodium oxide content with a mineralizer to obtain a mixed material;
[0008] The mixed material is calcined under a set temperature condition so that the mixed material is fully converted into a spherical α-alumina phase to obtain α-alumina.
[0009] Optionally, the set temperature is 1450°C to 1500°C.
[0010] Optionally, the target sodium oxide content is 0.03wt% to 0.07wt%.
[0011] Optionally, the industrial alumina is pretreated to obtain alumina having a target sodium oxide content, comprising:
[0012] CO2 is introduced into the industrial alumina slurry to obtain alumina with a target sodium oxide content.
[0013] Optionally, the CO2 inlet flow rate is 2200m 3 / h~3200m 3 / h, and / or the CO2 introduction time is 5min~7min.
[0014] Optionally, the CO2 introduction time is 5 minutes.
[0015] Optionally, the mineralizer includes boric acid.
[0016] Optionally, the weight of the mineralizer is 0.5% to 1% of the weight of the acid-washed alumina.
[0017] In a second aspect, the present application provides alpha alumina prepared by the method described in any one of the embodiments of the first aspect of claim.
[0018] Optionally, the α-alumina meets the following indicators: the sodium oxide content is less than 0.02%, the grain size D50 is 1.8
[0019] μm~2.2μm, the conversion rate is greater than 95%, and the morphology is spherical.
[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0021] The preparation method of the α-alumina provided in the embodiment of the present application comprises: pre-treating industrial alumina to obtain alumina with a target sodium oxide content; mixing the alumina with a target sodium oxide content with a mineralizer to obtain a mixed material; calcining the mixed material under a set temperature condition so that the mixed material is fully converted into a spherical α-alumina phase to obtain α-alumina. Pre-treating the industrial alumina slurry to obtain alumina with a target sodium oxide content can remove impurities in the industrial alumina slurry and preliminarily remove part of the sodium in the industrial alumina, while ensuring that the subsequent target α-alumina morphology is spherical; the mineralizer can promote the growth of grains in the α-alumina and adjust the crystal form to a spherical shape; under a set temperature condition, calcining the mixed material so that the spherical α-alumina phase is completely converted; the mineralizer cooperates with the calcination with a set temperature to further reduce the sodium oxide content in the α-alumina and adjust the microscopic morphology of the alumina, and finally obtains an α-alumina that takes into account both ultra-low sodium and spherical morphology. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1 A schematic flow chart of a method for preparing alpha alumina provided in an embodiment of the present application;
[0025] Figure 2 The microstructure of the α-alumina sample obtained by calcining at 1450° C. without adding a mineralizer after 5-minute acid washing provided in the embodiment of the present application;
[0026] Figure 3 The microstructure of the α-alumina sample obtained by calcining at 1500° C. without adding a mineralizer after 5-minute acid washing provided in the embodiment of the present application;
[0027] Figure 4 The microstructure of the α-alumina sample obtained by calcining at 1450° C. without adding a mineralizer after 7 minutes of pickling provided in the embodiment of the present application;
[0028] Figure 5 The microstructure of the α-alumina sample obtained by calcining at 1500° C. without adding a mineralizer after 7 minutes of pickling provided in the embodiment of the present application;
[0029] Figure 6 This is a microstructure diagram of α alumina obtained by calcining at 1450° C. after 5 minutes of pickling provided in the embodiment of the present application with 0.5% boric acid mineralizer added;
[0030] Figure 7 This is a microstructure diagram of α alumina obtained by calcining at 1450° C. after 5 minutes of pickling provided in the embodiment of the present application with 1% boric acid mineralizer added;
[0031] Figure 8 The microstructure of α alumina obtained by calcining at 1500° C. after 5 minutes of pickling provided in the embodiment of the present application with 0.5% boric acid mineralizer added;
[0032] Fig. 9 This is a microstructure diagram of α alumina obtained by calcining at 1500° C. after 5 minutes of acid washing with 0.5% boric acid mineralizer provided in the examples of the present application. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0034] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0035] In the present application, the terms "include", "comprises", etc. mean "including but not limited to". "And / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0036] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0037] In a first aspect, the present application provides a method for preparing alpha alumina. Figure 1 A schematic diagram of a process for preparing α-alumina provided in the embodiment of the present application; see Figure 1 , the method comprising:
[0038] S1. pretreating industrial alumina to obtain alumina with a target sodium oxide content;
[0039] In some embodiments, the target sodium oxide content is 0.03 wt % to 0.07 wt %.
[0040] In an embodiment of the present application, the industrial alumina slurry is pretreated to obtain alumina with a target sodium oxide content. Impurities in the industrial alumina slurry can be removed, and part of the sodium in the industrial alumina can be preliminarily removed to obtain alumina with a target sodium oxide content, while ensuring that the subsequent target α-alumina has a spherical morphology. Exemplarily, the above-mentioned target sodium oxide content can be 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, etc. In addition, the industrial alumina slurry can be obtained by: industrial alumina and deionized water are mixed at a solid content of 300g / L, and after CO2 washing, three times the water of the industrial alumina is used for washing.
[0041] In some embodiments, the pretreatment of industrial alumina to obtain alumina having a target sodium oxide content comprises:
[0042] CO2 is introduced into the industrial alumina slurry to obtain alumina with a target sodium oxide content.
[0043] In some embodiments, the CO2 inlet flow rate is 2200m 3 / h~3200m 3 / h, and / or the CO2 introduction time is 5min~7min.
[0044] In some embodiments, the CO2 is introduced for 5 minutes.
[0045] In the present embodiment, the acid-base neutralization pretreatment method is adopted, and the raw material slurry is washed with carbon dioxide gas without introducing impurities. The impurity sodium carbonate produced is washed and filtered with deionized water and then enters the mother liquor, thereby achieving the purpose of removing impurities. The CO2 inlet flow rate can be 2200m 3 / h~3200m 3 / h, and / or the CO2 injection time can be 5min to 7min, which can fully carry out the acid-base neutralization reaction, obtain alumina with a target sodium oxide content, and adjust the grain size of the pickled alumina, while saving energy consumption. For example, the CO2 injection flow rate can be 2200m 3 / h、2300m 3 / h、2400m 3 / h、2500m 3 / h、2600m 3 / h、2700m 3 / h、2800m 3 / h、2900m 3 / h、3000m 3 / h、3100m 3 / h、3200m 3 / h, etc., the introduction time can be 5min, 6min, 7min, etc., and further, the introduction time of CO2 can be 5min.
[0046] S2, mixing the alumina having the target sodium oxide content with a mineralizer to obtain a mixed material;
[0047] In some embodiments, the mineralizer comprises: boric acid.
[0048] In some embodiments, the weight of the mineralizer is 0.5% to 1% of the weight of the acid-washed alumina.
[0049] In the embodiment of the present application, the mineralizer may be boric acid, so as to promote the growth of grains in alpha alumina, and the weight of the mineralizer may be 0.5% to 2% of the weight of the pickled alumina, so as to avoid excessive use of the mineralizer, which may lead to aggravation of the crystal flakes and difficulty in obtaining the target spherical morphology. For example, the weight of the mineralizer may be 0.5%, 0.8%, 1%, etc. of the weight of the pickled alumina.
[0050] S3. Under a set temperature condition, the mixed material is calcined to fully transform the mixed material into a spherical α-alumina phase to obtain α-alumina.
[0051] In some embodiments, the set temperature is 1450°C to 1500°C.
[0052] In the embodiment of the present application, the above-mentioned set temperature can be 1450℃~1500℃ high temperature calcination to ensure complete crystal transformation, further adjust the grain size of α alumina, the conversion rate reaches more than 95%, and the mineralizer adjusts the crystal form into a spherical shape. Exemplarily, the above-mentioned set temperature can be 1450℃, 1460℃, 1470℃, 1480℃, 1490℃, 1500℃, etc. In addition, the calcination holding time can be 4h.
[0053] In a second aspect, the present application provides alpha alumina prepared by the method described in any embodiment of the first aspect of claim.
[0054] In some embodiments, the α-alumina meets the following indicators: a sodium oxide content of less than 0.02%, a grain size D50 of 1.8 μm to 2.2 μm, a conversion rate of greater than 95%, and a spherical morphology.
[0055] In the embodiment of the present application, after a series of impurity reduction treatments are performed on industrial alumina, a preferred mineralizer is introduced, and after high-temperature and long-term calcination, the purpose of calcining α-alumina for spherical ceramic substrate 96 porcelain with a sodium oxide content of less than 0.04% can be achieved.
[0056] The α alumina is realized based on the preparation method of the α alumina mentioned above. The specific steps of the preparation method of the α alumina can refer to the above embodiment. Since the α alumina adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0057] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0058] Add 150g of industrial alumina to a 500ml measuring cylinder, add deionized water to 500ml, stir evenly with a glass rod, and then pass CO2 gas into the cylinder at a flow rate of 2200m 3 / h; the ventilation time was controlled at 5min and 7min, filtered and washed with 3 times hot water, and then filtered and dried. Please refer to Table 1 for the composition results (wt%) of industrial alumina for the CO2 ventilation time.
[0059] Table 1 Composition results of industrial alumina during CO2 flow (wt%)
[0060] serial number <![CDATA[Duration of CO2 passage / min]]> <![CDATA[SiO2%]]> <![CDATA[Fe2O3%]]> <![CDATA[Na2O%]]> 1 0 0.013 0.008 0.278 2 5 0.013 0.008 0.063 3 7 0.01 0.008 0.034
[0061] It can be seen from Example 1 that the sodium oxide content of industrial alumina after 5min and 7min CO2 pickling can reach less than 0.07%.
[0062] Comparative Example 1
[0063] Add 150g of industrial alumina to a 500ml measuring cylinder, add deionized water to 500ml, stir evenly with a glass rod, and then pass CO2 gas into the cylinder at a flow rate of 2200m 3 / h; ventilation time is controlled at 5min and 7min, filtered and washed with 3 times hot water, and then filtered to dry the filter cake to obtain pickled alumina. 5min and 7min CO2 pickled alumina are calcined at 1450℃ and 1500℃ respectively without adding mineralizer, the insulation time is 4 hours, the 0-1000℃ heating rate is 10℃ / min, and the 1000-1450℃ / 1500℃ heating rate is 6℃ / min. Please refer to Table 2 for the indicators of α alumina obtained by calcining at 1450℃ and 1500℃ without adding mineralizer for 5min pickled alumina, and please refer to Table 2 for the indicators of α alumina obtained by calcining at 1450℃ and 1500℃ without adding mineralizer for 7min pickled alumina.
[0064] Table 2 Indexes of α-alumina obtained by calcining at 1450℃ and 1500℃ without adding mineralizer after 5min pickling
[0065]
[0066] Table 3 Indexes of α-alumina obtained by calcining at 1450℃ and 1500℃ without adding mineralizer after 7min pickling
[0067]
[0068] Figure 2 The microstructure of the α-alumina sample obtained by calcining at 1450° C. without adding a mineralizer after 5-minute acid washing provided in the embodiment of the present application; Figure 3 The microstructure of the α-alumina sample obtained by calcining at 1500°C without adding a mineralizer after 5 minutes of acid washing provided in the embodiment of the present application; see Figures 2-3 , indicating that after 5 minutes of pickling, alumina can be calcined at 1450℃ and 1500℃ respectively without adding mineralizer, and the grain size can reach 1.8-2.2μm, the α conversion rate is less than 95%, the spheroidization effect is not good, and some grains are melted and appear worm-like. Figure 4 The microstructure of the α-alumina sample obtained by calcining at 1450° C. without adding a mineralizer after 7 minutes of pickling provided in the embodiment of the present application; Figure 5 The microstructure of the α-alumina sample obtained by calcining at 1500°C without adding a mineralizer after 7 minutes of pickling provided in the embodiment of the present application; see Figures 4-5 , indicating that after 7 minutes of pickling, the alumina was calcined at 1450℃ and 1500℃ respectively without adding mineralizer. Although the sodium oxide content of α alumina was low, the grain size was not within the range of 1.8-2.2μm, the α conversion rate was less than 95%, and the spheroidization effect was not good.
[0069] Example 1
[0070] Add 150g of industrial alumina to a 500ml measuring cylinder, add deionized water to 500ml, stir evenly with a glass rod, and then pass CO2 gas into the cylinder at a flow rate of 2200m 3 / h; ventilation time is controlled at 5min, filtered and washed with 3 times hot water, and then filtered to dry the filter cake to obtain pickled alumina. 0.5% boric acid and 1% boric acid are added to the 5min pickled alumina respectively, and then calcined at 1450℃ and 1500℃ respectively, with a holding time of 4h, a 0-1000℃ heating rate of 10℃ / min, and a 1000-1450℃ / 1500℃ heating rate of 6℃ / min. Please refer to Table 4 for the indicators of α alumina obtained by calcining at 1450℃ and 1500℃ when a mineralizer is added to the 5min pickled alumina.
[0071] Table 4 Indices of α-alumina obtained by calcining at 1450℃ and 1500℃ with the addition of mineralizer after 5min pickling
[0072] name <![CDATA[SiO2%]]> <![CDATA[Fe2O3%]]> <![CDATA[Na2O%]]> α conversion rate % Grain size D50, μm 1450-5B 0.015 0.008 0.014 96.1 2.118 1450-10B 0.019 0.008 0.014 95.7 2.158 1500-5B 0.013 0.008 0.014 95.2 2.160 1500-10B 0.021 0.008 0.010 95.1 2.200
[0073] 5B means 0.5% boric acid, and 10B means 1% boric acid.
[0074] Figure 6 This is a microstructure diagram of α alumina obtained by calcining at 1450° C. after 5 minutes of pickling provided in the embodiment of the present application with 0.5% boric acid mineralizer added; Figure 7 This is a microstructure diagram of α alumina obtained by calcining at 1450° C. after 5 minutes of pickling provided in the embodiment of the present application with 1% boric acid mineralizer added; Figure 8 The microstructure of α alumina obtained by calcining at 1500° C. after 5 minutes of pickling provided in the embodiment of the present application with 0.5% boric acid mineralizer added; Fig. 9 The microstructure of α alumina obtained by calcining at 1500°C after 5 minutes of acid washing with 0.5% boric acid mineralizer provided in the embodiment of the present application; see Figures 6 to 9 , combined with Table 4, it is shown that the α-alumina obtained in the embodiment of the present application meets the following indicators: the sodium oxide content is less than 0.02%, the grain size is 1.8μm to 2.2μm, the conversion rate is greater than 95%, and the morphology is spherical. In particular, the spheroidization effect of 1450-5B is significant, and the grains are spherical.
[0075] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0076] (1) The present application example improves the quality of calcined α alumina, reduces the impurity content, and prepares spherical α alumina in a microscopic state;
[0077] (2) In the embodiment of the present application, after a series of impurity reduction treatments are performed on industrial alumina, a mineralizer is introduced, and after high-temperature and long-term calcination, a spherical ceramic substrate 96 ceramic calcined α alumina with a sodium oxide content of less than 0.02% can be obtained;
[0078] (3) In the embodiment of the present application, a CO2 ventilation method is used to pre-treat the raw alumina without introducing impurities to obtain an alumina raw material with a low sodium oxide content. A mineralizer and a high-temperature furnace static calcination method are then introduced to further remove impurities and adjust the microscopic morphology of the alumina to prepare a spherical calcined α-alumina product with a sodium oxide content of less than 0.02% and an original grain size of about 2 μm.
[0079] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing α-alumina, characterized in that: The method comprises: Pre-treating industrial alumina to obtain alumina with a target sodium oxide content; Mixing the alumina having a target sodium oxide content with a mineralizer to obtain a mixed material; The mixed material is calcined under a set temperature condition so that the mixed material is fully converted into a spherical α-alumina phase to obtain α-alumina.
2. The method according to claim 1, characterized in that The set temperature is 1450°C to 1500°C.
3. The method according to claim 1, characterized in that The target sodium oxide content is 0.03 wt % to 0.07 wt %.
4. The method according to claim 1, characterized in that: The process of pretreating industrial alumina to obtain alumina having a target sodium oxide content comprises: CO2 is introduced into the industrial alumina slurry to obtain alumina with a target sodium oxide content.
5. The method according to claim 4, characterized in that The CO2 inlet flow rate is 2200m 3 / h~3200m 3 / h, and / or the CO2 introduction time is 5min~7min.
6. The method according to claim 5, characterized in that The CO2 introduction time is 5 min.
7. The method according to claim 1, characterized in that The mineralizer includes boric acid.
8. The method according to any one of claims 1 to 7, characterized in that: The weight of the mineralizer is 0.5% to 1% of the weight of the acid-washed alumina.
9. Alpha alumina prepared by the method according to any one of claims 1 to 8.
10. The α-alumina according to claim 9, characterized in that The α-alumina meets the following indicators: the sodium oxide content is less than 0.02%, the grain size D50 is 1.8 μm to 2.2 μm, the conversion rate is greater than 95%, and the morphology is spherical.