Preparation method and application of surface phosphoric acid modified defective bismuth oxide nanosheet
By modifying the defective bismuth oxide nanosheets PO43-Bi2O3-x as catalysts loaded on the carbon felt electrode, the problem of low efficiency of traditional electrochemical uranium extraction materials in high concentration F-/U(VI) environment is solved, and the problem of low efficiency of traditional electrochemical uranium extraction materials is achieved. It has efficient uranium extraction and analysis, adapts to different pH conditions and interferes with ion interference, and has the advantages of efficient and long-term recycling.
Patent Information
- Application Number
- CN202411041795.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional electrochemical uranium extraction electrode materials are inefficient in high concentration F-/U(VI) environments and are difficult to adapt to different pH conditions and interfere with ion interference, limiting the efficient extraction of uranium in uranium production wastewater.
The surface phosphoric acid modification defective bismuth oxide nanosheets PO43-Bi2O3-x are used as catalysts to load on the carbon felt electrode. By electrochemical extraction of uranium, ammonium biphosphate and CTAB are used to precipitate and modify, so as to improve the binding capacity of UO2Fx and adapt to High F-concentration and different pH conditions.
It significantly improves the uranium extraction efficiency and analytical efficiency, can maintain efficient uranium extraction in a high F-concentration environment, adapt to different pH conditions, and has long-term recycling capabilities, and the uranium extraction efficiency reaches 4764.5 mg/g.
Smart Images

Figure CN118954589A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials, and in particular relates to a preparation method and application of surface phosphoric acid-modified defective bismuth oxide nanosheets. Background Art
[0002] As the basis of nuclear energy, uranium can only support the nuclear industry for less than a century. The shortage of uranium resources has put forward new requirements for improving uranium production efficiency. The recovery rate of residual uranium in the production vessel wastewater will directly affect the uranium production efficiency. Since uranium fluoride is widely used as an intermediate in the production vessel, the production vessel wastewater usually has high concentrations of uranium and fluoride ions. Uranium in the wastewater is in the form of soluble hexavalent uranyl (UO2 2+ , U(VI)) in the form of high concentration (>100 mg / L) and ultra-high concentration of F - (up to 30g / L) coexistence. Due to the complex uranium species and negatively charged complexes, traditional adsorption or ion exchange extraction methods have efficiency losses, as well as inevitable alkali metal impurities in the extraction products, which limit the uranium production efficiency. Electrochemical uranium extraction, as an alternative extraction strategy, converts U(VI) into insoluble crystalline products through coordination reduction, bringing new ideas to improve the uranium extraction efficiency in complex environments. Carbonaceous electrode materials can effectively extract uranium in uranium mine wastewater through electrochemistry, indicating that electrochemical uranium extraction can resist the interference of multiple cations. The design of traditional electrochemical uranium extraction electrode materials is to introduce functional groups that bind to U(VI). However, this is not suitable for the actual system of uranium production wastewater, because F in uranium production wastewater - The molar ratio of / U(VI) reaches 10 3 , the type of uranium belongs to UO2F x And with a lot of F - Therefore, it is necessary to rationally design a method that can enhance the UO2F x Combined electrode materials are used to electrochemically extract uranium from uranium production wastewater. Summary of the invention
[0003] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0004] In order to achieve these purposes and other advantages according to the present invention, a surface phosphoric acid modified defective bismuth oxide nanosheet PO4 is provided. 3- -Bi2O 3-x The preparation method is characterized by comprising:
[0005] Step 1: Add Bi(NO3)3·5H2O to ethylene glycol, then slowly add nitric acid, and then disperse by ultrasonic until Bi(NO3)3·5H2O is completely dissolved, evaporate the mixture to obtain a yellow viscous substance as a precursor, transfer the precursor to a muffle furnace for high-temperature oxidation, cool naturally, wash with ethanol and water, and then dry to obtain yellow Bi2O3 nanosheets;
[0006] Step 2: Mix water and ethanol to obtain a solvent, dissolve Bi2O3 nanosheets, Ca(NO3)2·4H2O, sodium hydroxide, and CTAB (hexadecyltrimethylammonium bromide) in the solvent, heat to obtain a mixture A, dissolve ammonium hydrogen phosphate in the solvent to obtain a mixture B, add the mixture B to the mixture A, keep warm, cool and precipitate in an ice water bath, collect the precipitate by centrifugation, wash it three times with the solvent, and then dry it to obtain bismuth oxide nanosheets PO4 modified with surface phosphoric acid 3- -Bi2O3;
[0007] Step 3: PO4 modified bismuth oxide nanosheets 3- -Bi2O3 is evenly spread on the crucible and placed in a plasma cleaner for cleaning for a period of time to obtain surface phosphoric acid-modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x .
[0008] Preferably, in step 1, the mass volume ratio of Bi(NO3)3·5H2O, ethylene glycol and nitric acid is 0.5-2g:20-60ml:1-4ml.
[0009] Preferably, in the step 1, the ultrasonic dispersion is performed for 5 to 20 minutes, the evaporation temperature is 180 to 220° C., the oxidation temperature is 350 to 450° C., the oxidation time is 4 to 8 hours, and the drying temperature is 55 to 80° C.
[0010] Preferably, in step 2, in mixture A, the volume ratio of water and ethanol in the solvent is 1-3:7-9, the mass volume ratio of Bi2O3 nanosheets, Ca(NO3)2·4H2O, sodium hydroxide, CTAB, and solvent is 0.5-2g:0.1-1g:0.1-1g:0.01-0.1g:10-50ml, and the heating temperature is 60-80°C.
[0011] Preferably, in step 2, in mixture B, the mass volume ratio of ammonium hydrogen phosphate to solvent is 0.1-1 g:10-50 ml.
[0012] Preferably, in the step 2, mixture B is added to mixture A at a rate of 0.5 to 2 ml / min at 70 to 80°C, the volume ratio of mixture A to mixture B is 1:1, the insulation temperature is 70 to 80°C, the mixture is placed for 0.5 to 2 hours, cooled and precipitated for 1 to 4 hours, the drying temperature is 50 to 70°C, and the drying time is 10 to 15 hours.
[0013] Preferably, the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The range of x is 0 to 3. In the step 3, the cleaning conditions are: in a H2 plasma environment, the power is 180 to 220 W, the pressure is 1 to 2 Pa, and the cleaning time is 25 to 45 minutes.
[0014] A defective bismuth oxide nanosheet PO4 modified by the above surface phosphoric acid 3- -Bi2O 3-x Surface phosphoric acid modified defective bismuth oxide nanosheets PO4 prepared by the preparation method 3- -Bi2O 3-x The application is characterized in that the defective bismuth oxide nanosheets PO4 are modified with surface phosphoric acid 3- -Bi2O 3-x The catalyst is loaded on a carbon felt electrode as a working electrode to electrochemically extract uranium from uranium-containing nuclear wastewater, including the following steps:
[0015] S1. Modify the prepared surface phosphoric acid-defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x As a catalyst, it was dispersed in a mixed solution of anhydrous ethanol and Nafion solution and ultrasonically treated to obtain a homogeneous catalyst solution. The carbon felt was ultrasonically treated with a mixture of ethanol and deionized water, and then the surface phosphoric acid was modified with defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x Loaded on carbon felt, in the conventional three-electrode system of the electrochemical workstation, the fluorine-containing uranium solution was used as the nuclear wastewater simulation solution, platinum wire and Ag / AgCl were used as the counter electrode and reference electrode respectively, and the carbon felt electrode was used as the working electrode to carry out electrochemical uranium extraction;
[0016] S2, placing the working electrode after uranium extraction in a nitric acid electrolyte, applying a constant positive potential, desorbing the working electrode, placing the desorbed working electrode in a simulated solution again, and conducting a cyclic uranium extraction experiment; then conducting an electrochemical uranium extraction experiment under different pH values and different interfering ions according to the method of S1;
[0017] S3. Prepare the working electrode according to the method of S1, and use real nuclear waste liquid to carry out actual nuclear waste water electrochemical uranium extraction experiment in a three-series electrolytic cell electrolysis device composed of a programmable power supply, an electrolysis unit and a control unit, wherein the electrolysis unit is composed of multiple electrolytic cells connected in series, and each electrolytic cell can be loaded with optimized electrode materials as required. The real nuclear waste liquid can enter the multi-stage series electrolytic cells through a pump, and the device will automatically perform waste liquid electrolysis according to pre-set parameters such as flow rate, current and voltage. The nuclear waste liquid flows through multiple electrolytic cells in turn, and the concentration of uranyl in the cells after electrolysis decreases in turn until the uranium concentration in the last electrolytic cell reaches the requirement and can be discharged from the electrolysis device.
[0018] Preferably, in S1, the mass volume ratio of the catalyst, anhydrous ethanol, and Nafion solution is 3-6 mg: 1-4 ml: 15-40 ul, the ultrasonic treatment time is 10-30 min, and the catalyst loading is fixed at 2-3 mg / cm 2 , the constant positive potential is 1~2V.
[0019] Preferably, in said S1, UO2 in the simulated solution 2+ Concentration ≥ 100 mg / L, F - Concentration ≥30g / L.
[0020] The present invention has at least the following beneficial effects:
[0021] (1) The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 of the present invention 3- -Bi2O 3-x It has a high uranium extraction efficiency. - The extraction capacity in uranium wastewater with a concentration of up to 30g / L reached 4764.5mg / g;
[0022] (2) The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 of the present invention 3- -Bi2O 3-x Has high parsing efficiency;
[0023] (3) The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 of the present invention 3- -Bi2O 3-x It has a high uranium extraction efficiency under different pH conditions and can be used for acidic wastewater produced by nuclear fuel element manufacturing and alkaline wastewater produced by uranium enrichment.
[0024] (4) The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 of the present invention 3- -Bi2O 3-x The extraction efficiency is still high in uranium wastewater with common interfering ions;
[0025] (5) The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 of the present invention 3- -Bi2O 3-x It can be used for uranium extraction and analysis multiple times and can be recycled for a long time.
[0026] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 prepared in Example 1 of the present invention 3- -Bi2O 3-x SEM images of
[0028] Figure 2 The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 prepared in Example 1 of the present invention 3- -Bi2O 3-x High-resolution transmission electron microscopy images of
[0029] Figure 3 The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 prepared in Example 1 of the present invention 3- -Bi2O 3-x EDX element mapping images;
[0030] Figure 4 The XRD patterns of Example 1 and Comparative Examples 1 to 3 of the present invention are shown below;
[0031] Figure 5 This is a graph of uranium extraction efficiency within 180 min of comparative examples 1 to 3 of application example 1 of the present invention;
[0032] Figure 6 The surface phosphoric acid-modified defective bismuth oxide nanosheet PO4 in Application Example 1 of the present invention is loaded 3- -Bi2O 3-x The deposition state of uranium on the carbon felt electrode at different times;
[0033] Figure 7 This is the application example 1 of the present invention: surface phosphoric acid modified defective bismuth oxide nanosheet PO4 3- -Bi2O 3-x Graph of desorption efficiency of uranium in 0.1M nitric acid desorption solution;
[0034] Figure 8 This is the application example 1 of the present invention: surface phosphoric acid modified defective bismuth oxide nanosheet PO4 3- -Bi2O 3-x Plots of uranium extraction efficiency and extracted mass with initial concentration;
[0035] Fig. 9 Surface phosphoric acid modified defective bismuth oxide nanosheets PO4 under different pH conditions in Example 1 of the present invention 3- -Bi2O 3-x Graph of uranium extraction efficiency;
[0036] Fig.10 For Application Example 1 of the present invention, - Surface phosphoric acid modified defective bismuth oxide nanosheets PO4 after adding different interfering ions in the presence of 3- -Bi2O 3-x Graph of uranium extraction efficiency;
[0037] Fig.11 This is the application example 1 of the present invention: surface phosphoric acid modified defective bismuth oxide nanosheet PO4 3- -Bi2O 3-x Graph of uranium extraction efficiency for recycling use;
[0038] Fig.12 This is an electrolysis device with three electrolytic cells connected in series according to Application Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0040] Example 1
[0041] A surface phosphoric acid-modified defective bismuth oxide nanosheet PO4 3- -Bi2O 3-x The preparation method comprises the following steps:
[0042] Step 1: Add 1g Bi(NO3)3·5H2O to 30ml ethylene glycol, then slowly add 2ml nitric acid, and then ultrasonically disperse for 10min until Bi(NO3)3·5H2O is completely dissolved, evaporate the mixture at 200°C, remove excess liquid, and obtain a yellow viscous substance as a precursor. Transfer the precursor to a muffle furnace and oxidize at 400°C for 6h. After natural cooling, wash with ethanol and water for 3 times, and then dry at 60°C to obtain yellow Bi2O3 nanosheets;
[0043] Step 2: Mix water and ethanol in a volume ratio of 3:7 to obtain a solvent, dissolve 1g Bi2O3 nanosheets, 0.5g Ca(NO3)2·4H2O, 0.3g sodium hydroxide, and 0.02g CTAB (hexadecyltrimethylammonium bromide) in 25ml of solvent, and heat to 75°C to obtain mixture A, dissolve 0.6g ammonium hydrogen phosphate in 40ml of solvent to obtain mixture B, and then add mixture B to mixture A at a rate of 1ml / min at 75°C according to a volume ratio of mixture A to mixture B of 1:1, keep warm at 75°C for 1h, then cool in an ice water bath and precipitate for 3h, collect the precipitate by centrifugation, wash it 3 times with a solvent, and then dry it at 60°C for 12h to obtain surface phosphoric acid-modified bismuth oxide nanosheets PO4 3- -Bi2O3;
[0044] Step 3: PO4 modified bismuth oxide nanosheets 3- -Bi2O3 was evenly spread on the crucible and placed in a plasma cleaner. In a H2 plasma environment, the cleaning was performed at a power of 200W and a pressure of 1Pa for 30 minutes. PO4 3- - The color of Bi2O3 nanosheet powder turns black, that is, surface phosphoric acid modified defective bismuth oxide nanosheet PO4 is obtained 3- -Bi2O 3-x .
[0045] Example 2
[0046] A PO4 with a surface phosphate defect 3- -Bi2O 3-x The method for preparing the nanosheet comprises the following steps:
[0047] Step 1: Add 1.5 g Bi(NO3)3·5H2O to 45 ml ethylene glycol, then slowly add 3 ml nitric acid, and then ultrasonically disperse for 10 min until Bi(NO3)3·5H2O is completely dissolved. Evaporate the mixture at 200 ° C, remove excess liquid, and obtain a yellow viscous substance as a precursor. Transfer the precursor to a muffle furnace and oxidize at 400 ° C for 6 h. After natural cooling, wash with ethanol and water for 3 times, and then dry at 60 ° C to obtain yellow Bi2O3 nanosheets.
[0048] Step 2: Mix water and ethanol in a volume ratio of 2:8 to obtain a solvent, dissolve 1.5 g Bi2O3 nanosheets, 0.8 g Ca(NO3)2·4H2O, 0.5 g sodium hydroxide, and 0.04 g CTAB (hexadecyltrimethylammonium bromide) in 30 ml of solvent, and heat to 75°C to obtain mixture A, dissolve 0.8 g ammonium hydrogen phosphate in 50 ml of solvent to obtain mixture B, and then add mixture B to mixture A at a rate of 1 ml / min at 75°C according to a volume ratio of mixture A to mixture B of 1:1, keep warm at 75°C for 1 hour, then cool in an ice water bath and precipitate for 3 hours, collect the precipitate by centrifugation, wash it 3 times with a solvent, and then dry it at 60°C for 12 hours to obtain surface phosphoric acid-modified bismuth oxide nanosheets PO4 3- -Bi2O3;
[0049] Step 3: PO4 with surface phosphate defects 3- -Bi2O3 nanosheets were evenly spread on the crucible and placed in a plasma cleaner. Under H2 plasma environment, the cleaning was carried out at a power of 200W and a pressure of 1Pa for 30min. PO4 3- - The color of Bi2O3 nanosheet powder turns black, that is, surface phosphoric acid modified defective bismuth oxide nanosheet PO4 is obtained 3- -Bi2O 3-x .
[0050] Comparative Example 1
[0051] The difference between this comparative example and Example 1 is that this comparative example only performs step 1 without performing subsequent steps, and finally obtains Bi2O3 nanosheets.
[0052] Comparative Example 2
[0053] The difference between this comparative example and Example 1 is that this comparative example performs steps 1 and 2 but does not perform step 3, and finally obtains bismuth oxide nanosheets PO4 modified with surface phosphoric acid. 3- -Bi2O3.
[0054] Comparative Example 3
[0055] The difference between this comparative example and Example 1 is that after obtaining Bi2O3 nanosheets in step 1, step 2 is not performed in this comparative example. Instead, the Bi2O3 nanosheets are evenly spread on the crucible, put into a plasma cleaning machine, and cleaned for 30 minutes at a power of 200 W and a pressure of 1 Pa in an H2 plasma environment. The color of the Bi2O3 nanosheet powder turns black, and finally Bi2O3 nanosheets are obtained. 3-x Nanosheets.
[0056] from Figure 1 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3--Bi2O 3-x It appears in the form of nanosheets; Figure 2 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The upper and lower plane spacings are 0.28nm and 0.32nm respectively; Figure 3 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x It is composed of Bi, O, and P elements uniformly; Figure 4 It can be seen that in the XRD graph, all samples show the characteristic peaks of Bi2O3, while the surface phosphoric acid-modified bismuth oxide nanosheets PO4 3- -Bi2O3 and surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x With additional Ca5(PO4)3(OH) signal, it is confirmed that PO4 3- The presence of groups.
[0057] Application Example 1
[0058] The surface phosphoric acid modified defective bismuth oxide nanosheets PO4 obtained in Example 1 3- -Bi2O 3-x The electrochemical performance test in simulated nuclear waste water includes the following steps:
[0059] S1. A 1×2 cm carbon felt was used as a carrier and subjected to ultrasonic treatment with a mixture of ethanol and deionized water. 5 mg of the surface phosphoric acid-modified defective bismuth oxide nanosheets PO4 prepared in Example 1 was added. 3- -Bi2O 3-x Dispersed in a mixed solution of 2 ml anhydrous ethanol and 30 μL Nafion solution, transferred and ultrasonicated for 20 min to obtain a homogeneous catalyst solution, and the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x Loaded on carbon felt, the loading amount is 2.5mg / cm 2 In a conventional three-electrode system on an electrochemical workstation (CHI660), the concentrations of U and F in 50 ml were UO2 2+ 100mg / L and F - In a 30 g / L high-fluorine and high-uranium solution, a platinum wire and Ag / AgCl were used as the counter electrode and reference electrode, respectively, to sample the surface phosphoric acid-modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The carbon felt electrode is used as the working electrode to complete the corresponding electrochemical uranium extraction.
[0060] S2, placing the working electrode after uranium extraction in a 0.1M nitric acid electrolyte, applying a constant positive potential of 1V, desorbing the working electrode, placing the desorbed working electrode again in a simulated solution, performing a cyclic electrochemical uranium extraction experiment, and performing electrochemical uranium extraction experiments at different pH values and different interfering ions;
[0061] S3, prepare the working electrode according to the method of S1, using Fig.12 The three-series electrolytic cell electrolysis device shown in the figure is used to carry out an actual electrochemical uranium extraction experiment from nuclear waste water, wherein the three-series electrolytic cell electrolysis device comprises ① a programmable power supply, ② an electrolysis unit and ③ a control unit, wherein ② the electrolysis unit is composed of a plurality of electrolytic cells connected in series, each electrolytic cell can be loaded with optimized electrode materials as required, ④ real nuclear waste liquid can enter the multi-stage series electrolytic cells through a pump, and according to the pre-set flow rate, current, voltage and other parameters, the device will automatically perform waste liquid electrolysis treatment, and the nuclear waste liquid will flow through a plurality of electrolytic cells in turn, and the concentration of uranyl in the cell after electrolysis will decrease in turn until the uranium concentration in the last electrolytic cell reaches the requirement and can be discharged from the electrolysis device.
[0062] from Figure 5 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The uranium extraction efficiency of Bi2O3, Bi2O3-x and surface phosphoric acid-modified bismuth oxide nanosheets PO4 3- -2 times, 1.7 times and 1.5 times of Bi2O3; Figure 6 It can be seen that during the uranium extraction process, light gray macroscopic crystals are modified with defective bismuth oxide nanosheets PO4 on the surface phosphoric acid. 3- -Bi2O 3-x The carbon felt electrode gradually grows and eventually turns yellow; Figure 7 It can be seen that after a typical electrochemical desorption process, the crystalline product was released into a dilute nitric acid solution, and the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The desorption efficiency of uranium is 95.1%; Figure 8 It can be seen that when the initial uranium concentration is within 50-500 mg / L, the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x It still has a high uranium extraction efficiency (>95%), with a maximum extraction capacity of 4764.5 mg / g. Fig. 9 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The uranium extraction efficiency in the pH range of 1 to 11 was >95%, indicating that the surface phosphoric acid modified defective bismuth oxide nanosheets PO43- -Bi2O 3-x Adaptability to uranium extraction in various situations, such as acidic wastewater from nuclear fuel element manufacturing and alkaline wastewater from uranium enrichment; Fig.10 It can be seen that with common interfering ions such as CO3 2- 、NO3 - , Cl - 、SO4 2- 、C2O4 2- and NH4 + The uranium extraction efficiency of Bi2O3 nanosheets decreased significantly, while the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x The extraction efficiency decreases minimally; Fig.11 It can be seen that the surface phosphoric acid modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x It worked well for 10 cycles of uranium extraction and desorption, indicating that it can be used cyclically for a long time.
[0063] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets, characterized in that: include: Step 1: Add Bi(NO3)3·5H2O to ethylene glycol, then slowly add nitric acid, and then disperse by ultrasonic until Bi(NO3)3·5H2O is completely dissolved, evaporate the mixture to obtain a yellow viscous substance as a precursor, transfer the precursor to a muffle furnace for high-temperature oxidation, cool naturally, wash with ethanol and water, and then dry to obtain yellow Bi2O3 nanosheets; Step 2: Mix water and ethanol to obtain a solvent, dissolve Bi2O3 nanosheets, Ca(NO3)2·4H2O, sodium hydroxide, and CTAB in the solvent, heat to obtain a mixture A, dissolve ammonium hydrogen phosphate in the solvent to obtain a mixture B, add the mixture B to the mixture A, keep warm, cool and precipitate in an ice water bath, collect the precipitate by centrifugation, wash it three times with the solvent, and then dry it to obtain bismuth oxide nanosheets PO4 modified with surface phosphoric acid 3- -Bi2O3; Step 3: PO4 modified bismuth oxide nanosheets 3- -Bi2O3 is evenly spread on the crucible and placed in a plasma cleaner for cleaning for a period of time to obtain surface phosphoric acid-modified defective bismuth oxide nanosheets PO4 3- -Bi2O 3-x .
2. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: In the step 1, the mass volume ratio of Bi(NO3)3·5H2O, ethylene glycol and nitric acid is 0.5-2g:20-60ml:1-4ml.
3. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: In the step 1, ultrasonic dispersion is performed for 5 to 20 minutes, the evaporation temperature is 180 to 220° C., the oxidation temperature is 350 to 450° C., the oxidation time is 4 to 8 hours, and the drying temperature is 55 to 80° C.
4. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: In the step 2, in the mixture A, the volume ratio of water and ethanol in the solvent is 1-3:7-9, the mass volume ratio of Bi2O3 nanosheets, Ca(NO3)2·4H2O, sodium hydroxide, CTAB, and solvent is 0.5-2g:0.1-1g:0.1-1g:0.01-0.1g:10-50ml, and the heating temperature is 60-80°C.
5. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: In the step 2, in the mixture B, the mass volume ratio of ammonium hydrogen phosphate to the solvent is 0.1-1 g:10-50 ml.
6. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: In the step 2, mixture B is added to mixture A at a rate of 0.5-2 ml / min at 70-80° C., the volume ratio of mixture A to mixture B is 1:1, the insulation temperature is 70-80° C., placed for 0.5-2 h, cooled and precipitated for 1-4 h, the drying temperature is 50-70° C., and the drying time is 10-15 h.
7. The method for preparing surface phosphoric acid-modified defective bismuth oxide nanosheets according to claim 1, characterized in that: The surface phosphoric acid modified defective bismuth oxide nanosheet PO4 3- -Bi2O 3-x The range of x is 0 to 3. In the step 3, the cleaning conditions are: in a H2 plasma environment, the power is 180 to 220 W, the pressure is 1 to 2 Pa, and the cleaning time is 25 to 45 minutes.
8. An application of a surface phosphoric acid-modified defective bismuth oxide nanosheet prepared by the method for preparing a surface phosphoric acid-modified defective bismuth oxide nanosheet according to any one of claims 1 to 7, characterized in that: The surface phosphoric acid modified defective bismuth oxide nanosheets are used as catalysts loaded on carbon felt electrodes as working electrodes to electrochemically extract uranium from uranium-containing nuclear wastewater, including: S1. Dispersing the prepared surface phosphoric acid-modified defective bismuth oxide nanosheets as a catalyst into a mixed solution of anhydrous ethanol and Nafion solution and ultrasonically treating the solution to obtain a homogeneous catalyst solution. Ultrasonic treating the carbon felt with a mixture of ethanol and deionized water. 3- -Bi2O 3-x Loaded on carbon felt, in the conventional three-electrode system of the electrochemical workstation, the electrochemical uranium extraction experiment was carried out with fluorine-containing and uranium-containing solution as the nuclear wastewater simulation solution, platinum wire and Ag / AgCl as the counter electrode and reference electrode respectively, and the carbon felt electrode as the working electrode; S2. Place the working electrode after uranium extraction in nitric acid electrolyte, apply a constant positive potential, desorb the working electrode, and place the desorbed working electrode again in the simulated solution to perform a cyclic uranium extraction experiment; then perform electrochemical uranium extraction experiments under different pH values and different interfering ions according to the method of S1.
9. The use of the surface phosphoric acid modified defective bismuth oxide nanosheets according to claim 8, characterized in that: In S1, the mass volume ratio of catalyst, anhydrous ethanol and Nafion solution is 3-6 mg: 1-4 ml: 15-40 ul, the ultrasonic treatment time is 10-30 min, and the catalyst loading is fixed at 2-3 mg / cm 2 , the constant positive potential is 1~2V.
10. The use of the surface phosphoric acid modified defective bismuth oxide nanosheets according to claim 8, characterized in that: In S1, UO2 in the simulated solution 2+ Concentration ≥ 100 mg / L, F - Concentration ≥30g / L.