Preparation method of negative electrode material for improving first charge-discharge efficiency and cycle performance
MoS2 was prepared by introducing polyvinyl alcohol and polydioxythiophene into MoS2 hydrothermal synthesis and adding sodium stearate, which solved the problem of MoS2 volume expansion and poor conductivity, and improved the cycle stability and charging of sodium ion batteries Discharge efficiency.
Patent Information
- Application Number
- CN202411004897.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
The application of graphite-like layered metal sulfide MoS2 in sodium ion batteries is affected by the problems of volume expansion and poor conductivity, which affects its stability and charge and discharge efficiency.
By introducing polyvinyl alcohol and polydioxythiophene during the hydrothermal synthesis of MoS2 and adding sodium stearate to form modified MoS2, combining binder and conductive agent, an efficient negative electrode material is prepared to inhibit volume expansion and increase the Conductivity.
The cycling stability and first charge and discharge efficiency of MoS2 are significantly improved, and the performance of sodium batteries is enhanced, especially the sodium ions produced after sodium stearate decomposition help to improve charge and discharge efficiency.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance. Background Art
[0002] Nowadays, society and the country are vigorously developing the new energy industry. Lithium batteries are favored by battery factory customers due to their large capacity and good cycle stability. However, from the cost point of view, lithium is relatively scarce, and the price of the negative electrode current collector copper foil of lithium batteries is relatively high. Therefore, the development of new low-cost, high-capacity batteries has become a general trend.
[0003] Currently, battery manufacturers are constantly developing new batteries, and sodium batteries have become a focus of attention. The graphite-like layered metal sulfide MoS2 is regarded as a potential negative electrode material for sodium-ion batteries due to its large interplanar spacing and excellent theoretical capacity. However, its volume expansion and poor conductivity make it difficult to use in practice. Therefore, how to improve the stability and conductivity of MoS2 has become a top priority.
[0004] In order to solve the above problems and improve the charging and discharging efficiency and cycle performance of the battery, the present invention provides a method for preparing a negative electrode material that improves the initial charging and discharging efficiency and cycle performance. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a negative electrode material that improves the initial charge and discharge efficiency and cycle performance, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0008] Step 1: Add thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate into pure water, stir evenly, bake, then wash with deionized water, and vacuum dry to obtain modified MoS2;
[0009] Step 2: Take the negative electrode active material modified MoS2, a binder, and a conductive agent, stir and mix them to obtain a slurry; apply the slurry on a carbon-coated aluminum foil, dry it, and obtain a negative electrode material.
[0010] More optimally, the mass ratio of the negative electrode active material: the binder: the conductive agent is (95-95.8): (2.8-4): (2-2.3).
[0011] More optimally, the molar ratio of thioacetamide to molybdenum trioxide is 1:2.
[0012] More optimally, the polyvinyl alcohol accounts for 1%-2% of the total mass of thioacetamide.
[0013] More optimally, the polydioxythiophene accounts for 0.5-1.5% of the total mass of thioacetamide.
[0014] More optimally, the sodium stearate accounts for 1%-5% of the total mass of thioacetamide.
[0015] More optimally, the binder is a mixture of sodium polyacrylate and carboxylated styrene-butadiene rubber.
[0016] More optimally, the conductive agent is SuperP.
[0017] More optimally, the mass ratio of the sodium polyacrylate to the carboxylated styrene-butadiene rubber is (6-10): (3-3.3).
[0018] More optimally, step 1: add thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate to pure water, stir evenly at 40-60°C, bake at 170-180°C for 16-18h, then wash with deionized water, and vacuum dry at 55-60°C for 22-24h to obtain modified MoS2;
[0019] Step 2: Take the negative electrode active material modified MoS2, a binder, and a conductive agent, stir and mix to obtain a slurry; apply the slurry on a carbon-coated aluminum foil, and dry it at 115-120°C for 10-12h to obtain the negative electrode material.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] (1) The present invention introduces polyvinyl alcohol and polydioxythiophene during the hydrothermal synthesis of MoS2. The coordinated use of polyvinyl alcohol and polydioxythiophene not only tightly coats the product MoS2 synthesized from thioacetamide and molybdenum trioxide, inhibits the volume expansion of MoS2 as a negative electrode during the charge and discharge process, and improves its cycle stability; but also polydioxythiophene has high conductivity, which can improve its initial charge and discharge efficiency.
[0022] (2) At the same time, the present invention adds a small amount of surfactant sodium stearate. After sodium stearate is decomposed by heat, it can not only improve the surface activity of the material, but also the sodium ions obtained by decomposition can improve the initial charge and discharge efficiency of sodium battery. The charge and discharge process of sodium ions obtained by decomposition of sodium stearate at the battery end at about 180°C is conducive to further improving the initial charge and discharge efficiency. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The manufacturers and models of the raw materials involved in the present invention are not particularly limited, and exemplarily include: molybdenum trioxide: particle size 10-40nm; sodium polyacrylate: model: 767418, which can be purchased from McLean; carboxylated styrene-butadiene rubber: Styronal7946, which can be purchased from BASF; conductive agent Super P: particle size 10-30nm; polyvinyl alcohol: model: 767382, which can be purchased from McLean; polydioxythiophene: polyethylene dioxythiophene, model: P913821, which can be purchased from McLean.
[0025] Embodiment 1: A method for preparing a negative electrode material for improving the initial charge and discharge efficiency and cycle performance, comprising the following steps:
[0026] Step 1: Preparation of modified MoS2:
[0027] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 50°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0028] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 2.5% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0029] Step 2: Preparation of negative electrode materials:
[0030] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0031] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0032] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0033] Example 2: The doping ratio of polydioxythiophene to thioacetamide is 0.5%, and the rest is the same as Example 1:
[0034] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0035] Step 1: Preparation of modified MoS2:
[0036] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 40°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0037] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 0.5% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0038] Step 2: Preparation of negative electrode materials:
[0039] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0040] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0041] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0042] Example 3: The doping ratio of polydioxythiophene to thioacetamide is 0.8%, and the rest is the same as Example 1:
[0043] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0044] Step 1: Preparation of modified MoS2:
[0045] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0046] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 0.8% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0047] Step 2: Preparation of negative electrode materials:
[0048] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0049] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0050] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0051] Example 4: The doping ratio of polydioxythiophene to thioacetamide is 1.3%, and the rest is the same as Example 1:
[0052] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0053] Step 1: Preparation of modified MoS2:
[0054] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0055] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 1.3% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0056] Step 2: Preparation of negative electrode materials:
[0057] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0058] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0059] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0060] Example 5: The doping ratio of polydioxythiophene to thioacetamide is 1.5%, and the rest is the same as Example 1:
[0061] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0062] Step 1: Preparation of modified MoS2:
[0063] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0064] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 1.5% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0065] Step 2: Preparation of negative electrode materials:
[0066] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0067] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0068] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0069] Example 6: The doping ratio of polydioxythiophene to thioacetamide is 0.5%, and the rest is the same as Example 1:
[0070] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0071] Step 1: Preparation of modified MoS2:
[0072] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0073] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 2.5% of the total mass of thioacetamide, sodium stearate accounts for 1% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0074] Step 2: Preparation of negative electrode materials:
[0075] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0076] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0077] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0078] Example 7: The doping ratio of polydioxythiophene to thioacetamide is 2%, and the rest is the same as Example 1:
[0079] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0080] Step 1: Preparation of modified MoS2:
[0081] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0082] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 2.5% of the total mass of thioacetamide, sodium stearate accounts for 2% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0083] Step 2: Preparation of negative electrode materials:
[0084] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0085] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0086] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0087] Example 8: The doping ratio of polydioxythiophene to thioacetamide is 4%, and the rest is the same as Example 1:
[0088] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0089] Step 1: Preparation of modified MoS2:
[0090] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0091] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 2.5% of the total mass of thioacetamide, sodium stearate accounts for 4% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0092] Step 2: Preparation of negative electrode materials:
[0093] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0094] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0095] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0096] Example 9: The doping ratio of polydioxythiophene to thioacetamide is 5%, and the rest is the same as Example 1:
[0097] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0098] Step 1: Preparation of modified MoS2:
[0099] Thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0100] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 2.5% of the total mass of thioacetamide, sodium stearate accounts for 5% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0101] Step 2: Preparation of negative electrode materials:
[0102] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0103] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0104] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0105] Comparative Example 1: No polydioxythiophene was added, and the rest was the same as Example 1:
[0106] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0107] Step 1: Preparation of modified MoS2:
[0108] Thioacetamide, molybdenum trioxide, polyvinyl alcohol and sodium stearate were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0109] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, sodium stearate accounts for 3.0% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0110] Step 2: Preparation of negative electrode materials:
[0111] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0112] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0113] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0114] Comparative Example 2: No sodium stearate was added, and the rest was the same as Example 1:
[0115] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0116] Step 1: Preparation of modified MoS2:
[0117] Thioacetamide, molybdenum trioxide, polyvinyl alcohol and polydioxythiophene were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0118] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, polydioxythiophene accounts for 0.5% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0119] Step 2: Preparation of negative electrode materials:
[0120] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0121] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0122] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0123] Comparative Example 3: No polydioxythiophene and sodium stearate were added, and the rest was the same as Example 1:
[0124] A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance comprises the following steps:
[0125] Step 1: Preparation of modified MoS2:
[0126] Thioacetamide, molybdenum trioxide and polyvinyl alcohol were added into pure water, stirred evenly at 60°C, and then baked in a forced air drying oven at 180°C for 16 hours, then washed with deionized water, and vacuum dried in a vacuum drying oven at 60°C for 24 hours to obtain modified MoS2;
[0127] The molar ratio of thioacetamide to molybdenum trioxide is 1:2, polyvinyl alcohol accounts for 3.5% of the total mass of thioacetamide, and the mass ratio of pure water to thioacetamide is 22:1;
[0128] Step 2: Preparation of negative electrode materials:
[0129] Take the negative electrode active material modified MoS2, the binder sodium polyacrylate and carboxyl styrene butadiene rubber, and the conductive agent Super P, stir and mix to obtain a slurry; coat the slurry on a carbon-coated aluminum foil, and dry it in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode material; the slurry coating thickness is 13 microns; the aluminum foil thickness is 14 microns;
[0130] The mass ratio of sodium polyacrylate to carboxylated styrene-butadiene rubber is 3:1;
[0131] The mass ratio of negative electrode active material modified MoS2: binder: conductive agent is 95:3:2.
[0132] experiment:
[0133] The negative electrode materials prepared in Examples 1-9 and Comparative Examples 1-3 were used for performance testing. The preparation of button batteries: the button battery shell was selected as CR2032 model, the diaphragm was selected as 20um diaphragm, and the pole pieces were respectively selected as the negative electrode materials prepared in Examples 1-9 and Comparative Examples 1-3. In a glove box filled with argon, the button batteries were assembled in the following order: battery shell - placing negative electrode piece - dripping electrolyte - placing diaphragm - dripping electrolyte - placing sodium sheet - placing gasket shrapnel - battery shell;
[0134] Button battery test: button battery charge and discharge tester (Wuhan Blue Electric, CT2001A) was used to perform charge and discharge test at 0.1A / g and 100 cycles test at 1A / g. The voltage range was 0-2.70V. The test results are shown in the following table:
[0135] serial number First charge and discharge efficiency Cycle performance Example 1 89.1% 96.2% Example 2 87.1% 91.8% Example 3 87.0% 91.5% Example 4 87.4% 91.9% Example 5 87.1% 91.4% Example 6 87.9% 89.0% Example 7 87.8% 88.8% Example 8 87.6% 88.4% Example 9 87.4% 87.1% Comparative Example 1 83.4% 68.1% Comparative Example 2 76.2% 71.0% Comparative Example 3 66.0% 56.5%
[0136] Conclusion: From the comparison of the data in the table, it can be seen that Examples 1-9 of the present invention introduce polyvinyl alcohol and polydioxythiophene in the hydrothermal synthesis process of MoS2. Polyvinyl alcohol and polydioxythiophene tightly coat the product MoS2 synthesized from thioacetamide and molybdenum trioxide, which inhibits the volume expansion of MoS2 as a negative electrode during the charge and discharge process, improves its cycle stability, and improves its first charge and discharge efficiency. Comparative Example 1 does not add polydioxythiophene, and the first charge and discharge efficiency and cycle performance are both reduced. Examples 1-9 of the present invention also add the surfactant sodium stearate. After sodium stearate is decomposed by heat, it can not only improve the surface activity of the material, but also the sodium ions obtained by decomposition can improve the first charge and discharge efficiency of sodium electricity. The charge and discharge process of sodium ions obtained by the decomposition of sodium stearate at the battery end at about 180°C is conducive to further improving the first charge and discharge efficiency. Comparative Example 2 does not add sodium stearate, and the first charge and discharge efficiency and cycle performance are reduced. Comparative Example 2 does not add polydioxythiophene and sodium stearate, and has the worst performance.
[0137] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a negative electrode material for improving the initial charge and discharge efficiency and cycle performance, characterized in that: The following steps are involved: Step 1: Add thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate into pure water, stir evenly, bake, then wash with deionized water and dry to obtain modified MoS2; Step 2: Take the negative electrode active material modified MoS2, a binder, and a conductive agent, stir and mix them to obtain a slurry; apply the slurry on a carbon-coated aluminum foil, dry it, and obtain a negative electrode material.
2. A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The mass ratio of the negative electrode active material: the binder: the conductive agent is (95-95.8): (2.8-4): (2-2.3).
3. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The molar ratio of thioacetamide to molybdenum trioxide is 1:
2.
4. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The polyvinyl alcohol accounts for 1%-2% of the total mass of thioacetamide.
5. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The polydioxythiophene accounts for 0.5-1.5% of the total mass of thioacetamide.
6. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The sodium stearate accounts for 1%-5% of the total mass of thioacetamide.
7. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The binder is a mixture of sodium polyacrylate and carboxyl styrene-butadiene rubber.
8. The method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: The conductive agent is Super P.
9. A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 7, characterized in that: The mass ratio of the sodium polyacrylate to the carboxylated styrene-butadiene rubber is (6-10):(3-3.3).
10. A method for preparing a negative electrode material for improving initial charge and discharge efficiency and cycle performance according to claim 1, characterized in that: Step 1: Add thioacetamide, molybdenum trioxide, polyvinyl alcohol, polydioxythiophene and sodium stearate to pure water, stir evenly at 40-60°C, bake at 170-180°C for 16-18h, then wash with deionized water, and vacuum dry at 55-60°C for 22-24h to obtain modified MoS2; Step 2: Take the negative electrode active material modified MoS2, a binder, and a conductive agent, stir and mix to obtain a slurry; apply the slurry on a carbon-coated aluminum foil, and dry it at 115-120°C for 10-12h to obtain the negative electrode material.