Tin bath process adjusting method for improving reflectivity of photo-thermal mirror

By adding metals such as silver, electrolytic iron and copper to the tin tank process, the FeO content in the photothermal ultra-white glass is reduced, the reflectivity of the photothermal mirror is improved, and the problem of difficult to reduce the FeO content in the photothermal ultra-white glass is solved. , achieving high reflectivity and low cost effects.

CN118954909APending Publication Date: 2024-11-15GANSU KAISHENG DAMING LIGHT ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085622.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The FeO content in the ultra-white light-thermal glass is difficult to reduce, which affects the reflectivity of the photothermal mirror and cannot meet the needs of high reflectivity.

Method used

In the tin tank process, X metal (silver), Y metal (electrolytic iron with a purity of 99.99%) and Z metal (copper) are added to the tin tank process to reduce the FeO content and increase the reflectivity of the photothermal mirror.

Benefits of technology

It effectively reduces the FeO content in the photothermal ultra-white glass, increases the reflectivity of the photothermal mirror, reduces the manufacturing cost, and promotes the quality of all-oxygen float method photothermal ultra-white glass and the development of energy-saving and environmentally friendly technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954909A_ABST
    Figure CN118954909A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of glass production, in particular to a tin bath process adjusting method for improving the reflectivity of a photo-thermal mirror. The invention relates to a tin bath process adjusting method for improving the reflectivity of a photo-thermal mirror, the process flow comprises the following steps: melting a batch, clarifying, homogenizing and cooling, polishing, solidifying, cooling and annealing, and after polishing, adding X metal at the rate of 0-0.025 kg / h, Y metal at the rate of 0-0.05 kg / h and Z metal at the rate of 0-0.1 kg / h into a tin liquid. A certain amount of X metal, Y metal and Z metal are added into the tin bath, and the metal activity of the X metal, the Y metal and the Z metal is higher than that of tin, so that the content of FeO in the photo-thermal ultra-white glass is reduced, the reflective rate of the photo-thermal ultra-white glass is increased, and the tinning amount is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass production, in particular to a tin bath process adjustment method for improving the reflectivity of a photothermal mirror. Background Art

[0002] With the accelerated construction of new energy systems, solar thermal power generation has the dual attributes of "power generation" and "energy storage", and can have the advantages of "absorption" and "peak regulation". It plays a vital role in building new power systems and has gradually become an important force in achieving the "dual carbon" goals. Solar thermal energy absorbs solar radiation through materials, which can produce different wavelengths, and then converts this light energy into heat energy to form a kind of energy with the function of heating. Therefore, the produced solar thermal glass has the function of gathering light energy and is widely used in industrial production and life. Solar thermal power generation refers to the process of focusing sunlight onto a solar energy collection device through a reflector, using solar energy to heat the heat transfer medium (liquid or gas) in the collection device, and then heating the water to form steam to drive or directly drive the generator to generate electricity.

[0003] The solar thermal glass used for solar thermal power generation is produced by the full oxygen float process. However, the solar thermal ultra-white glass produced by the full oxygen float process has always been troubled by the mutual influence of oxygen in the tin liquid and the FeO content in the glass. In order to meet the needs of solar thermal ultra-white glass power generation, the reflectivity of the solar thermal mirror is high (4mm solar thermal mirror reflectivity ≥ 94.5%). In order to improve the reflective performance of the solar thermal ultra-white glass, it is necessary to control the iron oxide content in the glass to not exceed 80ppm, and the FeO content in the glass should be reduced as much as possible. Therefore, it is particularly important to reduce the iron oxide content in the solar thermal ultra-white glass to improve the reflectivity of the solar thermal glass. Summary of the invention

[0004] In view of the existing problems, the present invention provides a tin bath process adjustment method for improving the reflectivity of the photothermal mirror, so as to solve the problem that the FeO content in the photothermal ultra-white glass cannot be reduced mentioned in the background technology.

[0005] In order to solve the existing problems, the present invention provides a tin bath process adjustment method for improving the reflectivity of a photothermal mirror, the process flow comprising: batch melting, clarification, homogenization cooling, polishing, solidification, cooling, and annealing, characterized in that: after polishing, X metal is added to the tin liquid at a rate of 0 to 0.025 kg / hour, Y metal at a rate of 0 to 0.05 kg / hour, and Z metal at a rate of 0 to 0.1 kg / hour.

[0006] Furthermore, the X metal is silver, the Y metal is electrolytic iron with a purity of 99.99%, and the Z metal is copper.

[0007] Furthermore, the batch material is melted by adding 2800-3000 kg of low-iron silica sand, 38-42 kg of alumina powder, 680-700 kg of low-iron dolomite, 275-300 kg of low-iron limestone, 900-920 kg of soda ash, 29-35 kg of sodium sulfate, 70-75 kg of potassium carbonate, 20-25 kg of sodium nitrate and 1400-1450 kg of broken glass into water accounting for 2.9% to 3.2% of the weight of the batch material, and then the batch material is added into a kiln and melted in a temperature range of 800-1000°C to obtain molten glass.

[0008] Furthermore, the clarification is that when the temperature of the glass liquid reaches 1400-1500°C, the viscosity of the glass liquid is about 10Pa.s. There are visible bubbles and dissolved gases in the glass liquid during the formation stage. As the temperature rises, the volume increases, the viscosity of the glass liquid decreases and a large amount of dissolved gas escapes until all the visible bubbles are discharged.

[0009] Furthermore, the homogenization cooling is performed by stirring evenly with a stirrer, and after cooling to 1100° C., the mixture flows into a tin bath.

[0010] Furthermore, the polishing is to achieve a balance between the glass liquid under the action of gravity and surface tension, so that the glass surface is smooth and flat, the flattening time is controlled at 1.7 minutes in the temperature field of 1000-1065°C, the longitudinal cooling rate is not more than 60°C / min, the first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

[0011] Furthermore, the solid state is that the temperature of the glass after the glass liquid is formed from the tin bath is 600-620°C.

[0012] Furthermore, the specific annealing operation is that the formed glass is passed through an annealing furnace to eliminate stress, the annealing temperature of zone A is 540-470°C, the annealing temperature of zone C is 480-380°C, and then it passes through the ret zone at 380-230°C and the annealing temperature of zone F at 380-230°C, and finally full oxygen ultra-white glass is obtained.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The present invention adds a certain amount of X metal, Y metal, and Z metal into the tin bath after polishing, and the metal activity of X metal, Y metal, and Z metal is stronger than that of tin, thereby reducing the content of FeO in the photothermal ultra-white glass and improving the reflectivity of the photothermal ultra-white glass.

[0015] 2. The tin bath adjustment process adopted by the present invention reduces manufacturing costs and the amount of tin infiltration, which has long-term economic significance and practical significance for sustainable development in improving the quality of all-oxygen combustion float thermal ultra-white glass and promoting new energy-saving and environmentally friendly technologies. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the process flow of the present invention; DETAILED DESCRIPTION

[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] See also Figure 1 A tin bath process adjustment method for improving the reflectivity of a photothermal mirror, the process flow includes: batch melting, clarification, homogenization cooling, polishing, solidification, cooling, annealing, after polishing, adding X metal to the tin liquid at a rate of 0 to 0.025 kg / hour, Y metal at a rate of 0 to 0.05 kg / hour, and Z metal at a rate of 0 to 0.1 kg / hour.

[0019] The X metal is silver, the Y metal is electrolytic iron with a purity of 99.99%, and the Z metal is copper.

[0020] After polishing, a certain amount of X metal, Y metal, and Z metal are added to the tin bath. The metal activity of X metal, Y metal, and Z metal is stronger than that of tin, which reduces the content of FeO in the photothermal ultra-white glass and improves the reflectivity of the photothermal ultra-white glass.

[0021] The mixing material is melted by adding 2800-3000 kg of low-iron silica sand, 38-42 kg of alumina powder, 680-700 kg of low-iron dolomite, 275-300 kg of low-iron limestone, 900-920 kg of soda ash, 29-35 kg of sodium sulfate, 70-75 kg of potassium carbonate, 20-25 kg of sodium nitrate and 1400-1450 kg of broken glass into water accounting for 2.9%-3.2% of the weight of the mixing material into a kiln, and then melting the mixing material in a temperature range of 800-1000°C to obtain glass liquid.

[0022] The clarification is when the temperature of the molten glass reaches 1400-1500°C, the viscosity of the molten glass is about 10Pa·s, and there are visible bubbles and dissolved gases in the molten glass during its formation stage. As the temperature rises, the volume increases, and the viscosity of the molten glass decreases, a large amount of gas escapes until all the visible bubbles are discharged.

[0023] The homogenization cooling is performed by stirring evenly with a stirrer, and then flowing into a tin bath after cooling to 1100°C.

[0024] Among them, the polishing is that the glass liquid reaches a balance under the action of gravity and surface tension, so that the glass surface is smooth and flat, the flattening time is controlled at 1.7 minutes in the temperature field of 1000-1065°C, the longitudinal cooling rate is not more than 60°C / min, the first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

[0025] The solid state is the glass formed by the glass liquid, and the temperature of the glass exiting the tin bath is 600-620°C.

[0026] Among them, the specific annealing operation is that the formed glass is passed through an annealing furnace to eliminate stress, the annealing temperature of zone A is 540-470°C, the annealing temperature of zone C is 480-380°C, and then it passes through the ret zone at 380-230°C and the annealing temperature of zone F at 380-230°C, and finally full oxygen ultra-white glass is obtained.

[0027] Embodiment 1:

[0028] The batch material is melted by adding 2.9% to 3.2% water by weight to a batch material consisting of 2900 kg of low-iron silica sand, 40 kg of alumina powder, 690 kg of low-iron dolomite, 290 kg of low-iron limestone, 910 kg of soda ash, 32 kg of sodium sulfate, 72.5 kg of potassium carbonate, 22.5 kg of sodium nitrate and 1425 kg of broken glass. After the batch material is put into the kiln, it is melted in the temperature range of 800 to 1000°C to obtain molten glass.

[0029] Clarification means that when the temperature of the molten glass reaches 1400-1500℃, the viscosity of the molten glass is about 10Pa·s. There are visible bubbles and dissolved gases in the molten glass during its formation stage. As the temperature rises and the volume increases, the viscosity of the molten glass decreases and a large amount of dissolved gas escapes until all the visible bubbles are discharged.

[0030] Homogenization cooling is to use a stirrer to stir evenly, and then flow into the tin bath after cooling to 1100℃.

[0031] Polishing is the process of achieving a balance between the glass liquid and the action of gravity and surface tension to make the glass surface smooth and flat. The flattening time is controlled at 1.7 minutes in a temperature field of 1000-1065°C, and the longitudinal cooling rate is not more than 60°C / min. The first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

[0032] Add metal X at a rate of 0 kg / hour, metal Y at a rate of 0 kg / hour, and metal Z at a rate of 0 kg / hour to the tin solution.

[0033] The solid state is the temperature of the glass after the glass liquid is formed and the glass exits the tin bath at 600-620℃.

[0034] The specific operation of annealing is that the glass after the glass liquid is formed passes through the annealing furnace to eliminate stress. The annealing temperature of zone A is 540~470℃, the annealing temperature of zone C is 480~380℃, and then it passes through the ret zone at 380~230℃, and the annealing temperature of zone F is 380~230℃, and finally full oxygen ultra-white glass is obtained.

[0035] Embodiment 2:

[0036] The batch material is melted by adding 2.9% to 3.2% water by weight to a batch material consisting of 2900 kg of low-iron silica sand, 40 kg of alumina powder, 690 kg of low-iron dolomite, 290 kg of low-iron limestone, 910 kg of soda ash, 32 kg of sodium sulfate, 72.5 kg of potassium carbonate, 22.5 kg of sodium nitrate and 1425 kg of broken glass. After the batch material is put into the kiln, it is melted in the temperature range of 800 to 1000°C to obtain molten glass.

[0037] Clarification means that when the temperature of the molten glass reaches 1400-1500℃, the viscosity of the molten glass is about 10Pa·s. There are visible bubbles and dissolved gases in the molten glass during its formation stage. As the temperature rises and the volume increases, the viscosity of the molten glass decreases and a large amount of dissolved gas escapes until all the visible bubbles are discharged.

[0038] Homogenization cooling is to use a stirrer to stir evenly, and then flow into the tin bath after cooling to 1100℃.

[0039] Polishing is the process of achieving a balance between the glass liquid and the action of gravity and surface tension to make the glass surface smooth and flat. The flattening time is controlled at 1.7 minutes in a temperature field of 1000-1065°C, and the longitudinal cooling rate is not more than 60°C / min. The first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

[0040] Add metal X at a rate of 0.0125 kg / hour, metal Y at a rate of 0.025 kg / hour, and metal Z at a rate of 0.05 kg / hour to the tin solution.

[0041] The solid state is the temperature of the glass after the glass liquid is formed and the glass exits the tin bath at 600-620℃.

[0042] The specific operation of annealing is that the glass after the glass liquid is formed passes through the annealing furnace to eliminate stress. The annealing temperature of zone A is 540~470℃, the annealing temperature of zone C is 480~380℃, and then it passes through the ret zone at 380~230℃, and the annealing temperature of zone F is 380~230℃, and finally full oxygen ultra-white glass is obtained.

[0043] Embodiment 3:

[0044] The batch material is melted by adding 2.9% to 3.2% water by weight to a batch material consisting of 2900 kg of low-iron silica sand, 40 kg of alumina powder, 690 kg of low-iron dolomite, 290 kg of low-iron limestone, 910 kg of soda ash, 32 kg of sodium sulfate, 72.5 kg of potassium carbonate, 22.5 kg of sodium nitrate and 1425 kg of broken glass. After the batch material is put into the kiln, it is melted in the temperature range of 800 to 1000°C to obtain molten glass.

[0045] Clarification means that when the temperature of the molten glass reaches 1400-1500℃, the viscosity of the molten glass is about 10Pa·s. There are visible bubbles and dissolved gases in the molten glass during its formation stage. As the temperature rises and the volume increases, the viscosity of the molten glass decreases and a large amount of dissolved gas escapes until all the visible bubbles are discharged.

[0046] Homogenization cooling is to use a stirrer to stir evenly, and then flow into the tin bath after cooling to 1100℃.

[0047] Polishing is the process of achieving a balance between the glass liquid and the action of gravity and surface tension to make the glass surface smooth and flat. The flattening time is controlled at 1.7 minutes in a temperature field of 1000-1065°C, and the longitudinal cooling rate is not more than 60°C / min. The first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

[0048] Add metal X at a rate of 0.025 kg / hour, metal Y at a rate of 0.05 kg / hour, and metal Z at a rate of 0.1 kg / hour to the tin solution.

[0049] The solid state is the temperature of the glass after the glass liquid is formed and the glass exits the tin bath at 600-620℃.

[0050] The specific operation of annealing is that the glass after the glass liquid is formed passes through the annealing furnace to eliminate stress. The annealing temperature of zone A is 540~470℃, the annealing temperature of zone C is 480~380℃, and then it passes through the ret zone at 380~230℃, and the annealing temperature of zone F is 380~230℃, and finally full oxygen ultra-white glass is obtained.

[0051]

[0052]

[0053] From the above, it can be concluded that a certain amount of X metal, Y metal, and Z metal are added to the tin bath after polishing, and the metal activity of X metal, Y metal, and Z metal is stronger than that of tin, thereby reducing the content of FeO in the photothermal ultra-white glass and improving the reflectivity of the photothermal ultra-white glass.

[0054] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A tin bath process adjustment method for improving the reflectivity of a photothermal mirror, the process flow comprising: The batch material is melted, clarified, homogenized and cooled, polished, solidified, cooled and annealed, characterized in that: after polishing, metal X is added to the tin liquid at a rate of 0 to 0.025 kg / hour, metal Y at a rate of 0 to 0.05 kg / hour, and metal Z at a rate of 0 to 0.1 kg / hour.

2. The tin bath process adjustment method for improving the reflectivity of the photothermal mirror according to claim 1 is characterized in that: The X metal is silver, the Y metal is electrolytic iron with a purity of 99.99%, and the Z metal is copper.

3. The tin bath process adjustment method for improving the reflectivity of the photothermal mirror according to claim 1 is characterized in that: The batch material is melted by adding 2900 kg of low-iron silica sand, 40 kg of alumina powder, 690 kg of low-iron dolomite, 290 kg of low-iron limestone, 910 kg of soda ash, 32 kg of sodium sulfate, 72.5 kg of potassium carbonate, 22.5 kg of sodium nitrate and 1425 kg of broken glass into water accounting for 2.9% to 3.2% of the weight of the batch material, and then putting the batch material into a kiln, and then melting it in the temperature range of 800 to 1000° C. to obtain glass liquid.

4. The tin bath process adjustment method for improving the reflectivity of the photothermal mirror according to claim 1 is characterized in that: The clarification is when the temperature of the glass liquid reaches 1400-1500°C, the viscosity of the glass liquid is about 10Pa.s, and there are visible bubbles and dissolved gases in the glass liquid during its formation stage. As the temperature rises, the volume increases, the viscosity of the glass liquid decreases and a large amount of dissolved gas escapes until all the visible bubbles are discharged.

5. The method for adjusting the tin bath process for improving the reflectivity of the photothermal mirror according to claim 1, characterized in that: The homogenization cooling is performed by stirring evenly with a stirrer, and then flowing into a tin bath after cooling to 1100°C.

6. The method for adjusting the tin bath process for improving the reflectivity of the photothermal mirror according to claim 1, characterized in that: The polishing is to achieve a balance between the glass liquid under the action of gravity and surface tension, so that the glass surface is smooth and flat. The flattening time is controlled at 1.7 minutes in the temperature field of 1000-1065°C, and the longitudinal cooling rate is not more than 60°C / min. The first pair of edge drawing machines are arranged at 9-10 meters of the 600-ton tin bath, and the temperature is at 930°C.

7. The method for adjusting the tin bath process for improving the reflectivity of the photothermal mirror according to claim 1, characterized in that: The solid state is that the temperature of the glass after the glass liquid is formed from the tin bath is 600-620°C.

8. The method for adjusting the tin bath process for improving the reflectivity of the photothermal mirror according to claim 1, characterized in that: The specific annealing operation is that the formed glass is passed through an annealing furnace to eliminate stress, the annealing temperature of zone A is 540-470°C, the annealing temperature of zone C is 480-380°C, and then it passes through the ret zone at 380-230°C and the annealing temperature of zone F at 380-230°C, and finally full oxygen ultra-white glass is obtained.