High-strength antibacterial glass and preparation method thereof
Through the three-step ion exchange method, the stress distribution of glass is regulated, the mechanical properties and antibacterial properties of antibacterial glass are improved, and the safety hazards caused by excessive tension in the glass in the prior art are solved, thus achieving high strength and high permeability rate effect.
Patent Information
- Application Number
- CN202410958988.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
AI Technical Summary
During the first step of ion exchange, existing ion exchange antibacterial glasses can easily lead to excessive tension in the glass, increasing the risk of crack propagation, and thus affecting the strength and safety of the glass.
The three-step ion exchange method is adopted. The first step is to use potassium nitrate and sodium nitrate mixed molten salt for ion exchange, the second step is to use pure potassium nitrate for ion exchange, and the third step is to use cesium nitrate and silver nitrate mixed molten salt for ion exchange, By regulating temperature and time, the surface compressive stress is established and the internal tension stress is reduced, and the mechanical properties and antibacterial properties of the glass are improved.
It effectively reduces the risk of cracking inside the glass, improves the mechanical properties and antibacterial properties of the glass, and avoids the conversion of silver ions into metal Ag, reduces the color changes of the glass, and improves the transmittance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass processing, and in particular to a high-strength antibacterial glass and a preparation method thereof. Background Art
[0002] With the continuous advancement of information display technology, the application field of touch screen panels is becoming increasingly wide, covering not only smart devices such as smartphones and bracelets, but also wider fields such as automotive display panels. However, the oil and sweat secreted from fingers provide a good environment for the reproduction and growth of bacteria, posing a greater safety hazard to people's health. Therefore, the demand for antibacterial glass is increasing.
[0003] Antibacterial glass can be divided into many types, such as soluble antibacterial glass, porous antibacterial glass, coated antibacterial glass and ion exchange antibacterial glass. Among them, ion exchange antibacterial glass combines high antibacterial properties, high transmittance and high strength, and has broad application prospects. The common antibacterial ions of ion exchange antibacterial glass are mainly Ag. + , Cu 2+ and Zn 2+ etc., among which Ag + The bactericidal effect is second only to Hg 2+ But Hg 2+ It has high toxicity and has now been eliminated, so silver-loaded antibacterial glass with strong antibacterial properties and non-toxicity has made great progress.
[0004] Existing ion exchange antibacterial glass usually needs to undergo a two-step ion exchange process. The first step is to exchange the glass with pure potassium nitrate molten salt or a mixed molten salt of sodium nitrate and potassium nitrate to obtain a higher strength; the second step is to exchange the glass with a mixed molten salt of potassium nitrate and silver nitrate to introduce Ag. + In the first step of ion exchange, K in the molten salt + Replace Na in glass + , through the "crowding" effect, a certain depth of compressive stress is formed on the glass surface. When the glass is subjected to external force, the external force must first overcome the surface compressive stress to put the glass in a tensile stress state, thereby improving the strength of the glass. On the other hand, the existence of the stress layer can inhibit the expansion of cracks, increase the energy required for crack expansion, and is also beneficial to improving the strength of the glass. In order to make the glass obtain a higher stress after the first step of ion exchange, the K in the molten salt is usually + The content is high. When the molten salt is pure potassium nitrate, the stress obtained after ion exchange is the largest. + An increase in the content is beneficial to increasing the surface compressive stress, but at the same time a large tensile stress will be generated inside the glass. When the tensile stress is large enough, once a crack is triggered, it will cause the glass to break and shatter into fine particles, posing a major safety hazard. Summary of the invention
[0005] The purpose of the present invention is to effectively achieve high strength and high ion exchange performance of glass through reasonable regulation of the ion exchange process. In view of the above-mentioned shortcomings of the prior art, a method for preparing high-strength antibacterial glass is proposed.
[0006] A method for preparing high-strength antibacterial glass comprises the following steps: S1, mixing potassium nitrate and sodium nitrate and heating them to obtain molten salt A; S2, preheating the cleaned glass sheet, and then immersing it in molten salt A to perform the first step of ion exchange; S3, heating potassium nitrate to obtain molten salt B, cleaning and preheating the glass after ion exchange in step S2, and then immersing it in molten salt B for the second step of ion exchange; S4, mixing cesium nitrate and silver nitrate and heating them to obtain molten salt C; S5. Clean and preheat the glass after ion exchange in step S3, and then immerse it in molten salt C for the third step of ion exchange to obtain high-strength antibacterial glass.
[0007] The above technical solution is further configured as follows: the first ion exchange temperature in step S2 is 440-460° C., and the ion exchange time is 4-8 hours.
[0008] The above technical solution is further configured as follows: the second step ion exchange temperature in step S3 is 420-440° C., and the ion exchange time is 0.5-2 h.
[0009] The above technical solution is further configured as follows: the mass percentage of potassium nitrate in the molten salt B is: the ion exchange temperature in the third step is 380-420° C., and the ion exchange time is 3-15 min.
[0010] The above technical solution is further configured as follows: the second step ion exchange temperature is lower than the first step ion exchange temperature, and the third step ion exchange temperature is lower than the second step ion exchange temperature.
[0011] The above technical solution is further configured as follows: the mass percentage of sodium nitrate in the molten salt A is 20-40%, and the mass percentage of potassium nitrate is 60-80%.
[0012] The above technical solution is further configured as follows: the mass percentage of cesium nitrate in the molten salt C is 98-99.5%, and the mass percentage of silver nitrate is 0.05-2%.
[0013] The beneficial effects of the present invention are: 1. The present invention improves the mechanical properties and antibacterial properties of glass through a three-step ion exchange method, specifically: through the first step of ion exchange of mixed molten salts of potassium nitrate and sodium nitrate, a certain surface compressive stress can be established while reducing the internal tensile stress of the glass, thereby reducing the risk of cracking of the glass from the inside; through the second step of ion exchange of pure potassium nitrate, the surface compressive stress of the glass can be further increased, thereby improving its mechanical properties; in the third step, the surface compressive stress of the glass can be further increased through ion exchange of cesium nitrate, and the antibacterial properties of the glass can be given through ion exchange of silver nitrate.
[0014] 2. The first step of ion exchange in this application uses K + and Na + and mixed molten salt, Na + The mass percentage is 20-40%, and the first step of ion exchange uses a higher temperature and a longer ion exchange time, which can obtain a deeper stress layer depth, thus affecting the interior of the glass. The higher Na + ratio, which can reduce K + The tensile stress generated inside the glass is reduced, so that in the first step of ion exchange, a certain surface compressive stress is established while reducing the tensile stress inside the glass, thereby reducing the risk of cracking from the inside of the glass; the second step of ion exchange uses pure potassium nitrate ion exchange, the ion exchange temperature and time are short, and K + Replace the Na on the glass surface after the first step of ion exchange + , further increasing the compressive stress on the glass surface without increasing the tensile stress inside the glass; the third step of ion exchange uses a mixed molten salt of cesium nitrate and silver nitrate. The ion exchange time is only 3-15 minutes. Through a short period of ion exchange, silver ions can be introduced into the glass surface while avoiding the probability of silver ions turning into metallic Ag, thereby reducing the color of the glass and improving the transmittance of the glass.
[0015] 3. The present invention generates three ion exchange layers on the glass surface through a three-step ion exchange reaction. The pressure of the three ion exchange layers on the glass should gradually increase. While ensuring that the pressure on the glass surface is relatively large, the large compressive stress difference between the glass surface and the interior of the glass leads to an increase in the tensile stress inside the glass, thereby making the glass have good mechanical properties. DETAILED DESCRIPTION
[0016] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.
[0017] Embodiment 1: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0018] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0019] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0020] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0021] Embodiment 2: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 40% sodium nitrate and 60% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0022] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0023] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0024] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0025] Embodiment 3: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0026] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0027] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 25 min.
[0028] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0029] Embodiment 4: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0030] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0031] (3) In terms of mass percentage, 99.7% cesium nitrate and 0.3% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0032] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0033] Embodiment 5: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 440°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0034] (2) Heat pure potassium nitrate molten salt to 420°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0035] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 415°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0036] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0037] Embodiment 6: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 8 hours.
[0038] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0039] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0040] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0041] Example 7 A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0042] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 3 hours.
[0043] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0044] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0045] Embodiment 8: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0046] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0047] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 380°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0048] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0049] Comparative Example 1: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) Pure potassium nitrate was heated to 460°C and a glass slide was immersed in it for the first step of ion exchange for 4 h.
[0050] (2) Heat pure potassium nitrate molten salt to 440°C and immerse the glass piece exchanged in the first step into it for the second step of ion exchange. The exchange time is 2 hours.
[0051] (3) In terms of mass percentage, 99.8% cesium nitrate and 0.2% silver nitrate were mixed evenly, heated to 420°C, and the glass piece obtained in the second step of ion exchange was immersed in the mixture for the third step of ion exchange. The exchange time was 15 min.
[0052] (4) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0053] Comparative Example 2: A method for preparing high-strength antibacterial glass, characterized in that it comprises the following steps: (1) In terms of mass percentage, 20% sodium nitrate and 80% potassium nitrate were mixed evenly, heated to 460°C, and a glass sheet was immersed in the mixture for the first step of ion exchange. The exchange time was 4 hours.
[0054] (2) After the first step of ion exchange, the glass sheet was not subjected to the second step of ion exchange, but was directly immersed in a mixed molten salt of 99.8% cesium nitrate and 0.2% silver nitrate at 420°C for 15 min.
[0055] (3) Take out the glass piece after ion exchange to obtain high-strength antibacterial glass.
[0056] The performance of Examples 1-8 and Comparative Examples 1-2 prepared above was tested, and the ion exchange conditions and test results are listed in Tables 1 and 2. The antibacterial performance is tested according to the JC / T 1054-2007 standard requirements.
[0057] Table 1: project Example 1 Example 2 Example 3 Example 4 Example 5 First step molten salt mass percentage (%) <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[40NaNO 3 +60KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> First step ion exchange temperature and time (℃ / h) 460 / 4 460 / 4 460 / 4 460 / 4 440 / 4 Second step ion exchange temperature and time (℃ / h) 440 / 2 440 / 2 440 / 2 440 / 2 420 / 2 The third step is the mass percentage of molten salt (%) <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <h2 style=";text-align:left;direction:ltr"><![CDATA[99.7CsNO <h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +0.3AgNO<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> The third step ion exchange temperature and time (℃ / min) 420 / 15 420 / 15 420 / 25 420 / 15 415 / 15 Surface compressive stress after the first step of ion exchange (MPa) 611 588 612 611 598 Depth of stress layer after first step ion exchange (μm) 11.9 9.1 12.1 12.6 9.7 Central tensile stress after the first step of ion exchange (MPa) 26 19 27 28 21 Surface compressive stress after the second step ion exchange (MPa) 628 595 627 627 604 Depth of stress layer after the second step ion exchange (μm) 13.0 9.6 12.9 13.1 10.2 Surface compressive stress after the third step ion exchange (MPa) 639 612 644 633 612 Step 3: Depth of stress layer after ion exchange (μm) 13.5 10.6 14.2 13.1 10.8 Escherichia coli antibacterial rate (%) 99.1 99.1 99.9 99.9 99.2 Table 2: project Example 6 Example 7 Example 8 Comparative Example 1 Comparative Example 2 First step molten salt mass percentage (%) <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> <![CDATA[100KNO 3 ]]> <![CDATA[20NaNO 3 +80KNO 3 ]]> First step ion exchange temperature and time (℃ / h) 460 / 8 460 / 4 460 / 4 460 / 4 460 / 4 Second step ion exchange temperature and time (℃ / h) 440 / 2 440 / 3 440 / 2 440 / 2 / The third step is the mass percentage of molten salt (%) <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> <![CDATA[99.8CsNO 3 +0.2AgNO 3 ]]> The third step ion exchange temperature and time (℃ / min) 420 / 15 420 / 15 380 / 15 420 / 15 420 / 15 Surface compressive stress (CS) after the first step of ion exchange 601 612 614 636 612 Depth of stress layer (DOL) after first step ion exchange 14.2 12.2 12.3 14.9 12.4 Central tensile stress after the first step of ion exchange (MPa) 30 27 27 36 28 Surface compressive stress (CS) after the second step ion exchange 611 639 630 641 / Depth of stress layer (DOL) after the second step ion exchange 16.1 13.9 13.1 15.3 / Surface compressive stress after the third step ion exchange (MPa) 620 645 631 648 614 Step 3: Depth of stress layer after ion exchange (μm) 16.6 14.3 13.3 15.8 12.6 Escherichia coli antibacterial rate (%) 99.0 99.1 98.2 99.1 99.0 The invention prepares a high-strength antibacterial glass by optimizing and adjusting the ion exchange process.
[0058] It can be seen from Examples 1-2 in Table 1 that as the sodium nitrate content in the molten salt A increases, the surface compressive stress and stress layer depth of the first step ion exchange decrease. The reason is that the potassium nitrate content in the molten salt decreases, and the potassium nitrate diffused into the glass + The decrease in the content of sodium nitrate causes the surface compressive stress and the depth of the stress layer to decrease. In particular, with the increase in the sodium nitrate content, the central tensile stress after the first step of ion exchange is significantly reduced. After the second step of ion exchange, the surface compressive stress increases. This is mainly due to the K in the molten salt. + Further replace Na in glass + The compressive stress formed is further increased. After the third step of ion exchange, the surface compressive stress is further increased, mainly due to Cs + With K + The radius difference is large, and the "congestion effect" is more obvious.
[0059] It can be seen from Examples 3-4 in Table 1 that with the extension of the third step ion exchange time and the increase of the silver nitrate content, the antibacterial property of the glass is significantly improved, mainly because with the increase of the silver nitrate content in the molten salt and the extension of the ion exchange time, more Ag + Spread over the glass surface.
[0060] As can be seen from Example 5 in Table 1, when the ion exchange temperature in the first step is reduced, the surface compressive stress and the stress layer depth are significantly reduced, and the central tensile stress is also reduced. When the ion exchange temperature in the second step is reduced, the surface compressive stress and the stress layer depth are also reduced.
[0061] It can be seen from Example 6 in Table 2 that, compared with Example 1, the surface compressive stress after the first step of ion exchange is reduced and the stress layer depth is increased. The reason is that the ion exchange time of Example 6 is increased and stress relaxation occurs in the glass during the exchange process.
[0062] It can be seen from Example 7 in Table 2 that when the ion exchange temperature in the second step increases, the compressive stress on the glass surface and the depth of the stress layer increase to a greater extent.
[0063] It can be seen from Example 8 in Table 2 that when the ion exchange temperature in the third step is reduced, the antibacterial property of the glass is significantly reduced.
[0064] It can be seen from Comparative Example 1 in Table 2 that when the first-step ion exchange molten salt contains only pure potassium nitrate, the surface compressive stress and exchange layer depth after the first-step ion exchange are both high, but the central tensile stress also increases significantly, and the risk of glass breakage increases.
[0065] It can be seen from Comparative Example 2 in Table 2 that when the glass is not subjected to the second step ion exchange, the surface compressive stress and stress layer depth of the final glass are both relatively low.
[0066] For matters not mentioned above, the prior art applies.
[0067] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing high-strength antibacterial glass, characterized in that: The steps include: S1, mixing potassium nitrate and sodium nitrate and heating them to obtain molten salt A; S2, preheating the cleaned glass sheet, and then immersing it in molten salt A to perform the first step of ion exchange; S3, heating potassium nitrate to obtain molten salt B, cleaning and preheating the glass after ion exchange in step S2, and then immersing it in molten salt B for the second step of ion exchange; S4, mixing cesium nitrate and silver nitrate and heating them to obtain molten salt C; S5. Clean and preheat the glass after ion exchange in step S3, and then immerse it in molten salt C for the third step of ion exchange to obtain high-strength antibacterial glass.
2. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The first ion exchange temperature in step S2 is 440-460° C., and the ion exchange time is 4-8 hours.
3. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The second step ion exchange temperature in step S3 is 420-440° C., and the ion exchange time is 0.5-2 h.
4. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The temperature of the third step ion exchange is 380-420° C., and the time of the ion exchange is 3-15 min.
5. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The second step ion exchange temperature is lower than the first step ion exchange temperature, and the third step ion exchange temperature is lower than the second step ion exchange temperature.
6. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The mass percentage of sodium nitrate in the molten salt A is 20-40%, and the mass percentage of potassium nitrate is 60-80%.
7. The method for preparing a high-strength antibacterial glass according to claim 1, characterized in that: The mass percentage of cesium nitrate in the molten salt C is 98-99.5%, and the mass percentage of silver nitrate is 0.05-2%.
8. A high-strength antibacterial glass, characterized in that: The high-strength antibacterial glass is prepared by the preparation method of any one of claims 1-8.
Citation Information
Patent Citations
Coated glass substrate or glass ceramic substrate with resistant multi-functional surface properties, method for production thereof and use thereof
CN107074621A
Chemical strengthening method for reducing warpage of glass and improving impact resistance of glass
CN110194599A
Preparation method of antibacterial glass
CN114195404A
Antimicrobial glass articles and methods of making and using same
US20140370303A1
Aluminosilicate glass, antibacterial glass and preparation method therefor
WO2017201681A1