DOPO phosphamide derivative flame retardant, preparation method thereof and application of DOPO phosphamide derivative flame retardant in waterborne polyurethane

By introducing DOPO phosphoramide derivative flame retardant into polyurethane, the synergistic effect of nitrogen and phosphorus has been used to solve the problems of flammability and toxic gas release of polyurethane, and efficient flame retardant performance has been achieved, especially significantly improved in water-based polyurethane. security.

CN118955564AActive Publication Date: 2024-11-15ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202410907307.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-15
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Polyurethane materials are flammable and release of toxic gases under high temperature or fire conditions, which poses a threat to people and the environment, especially in water-based polyurethanes, with the lack of effective flame retardant solutions.

Method used

By combining para-aminophene with benzyl chloride, a double-terminal hydroxyl structure is introduced and reacted with DOPO to prepare halogen-free, smoke-free, non-toxic DOPO phosphoramide derivative flame retardant, which is involved in aqueous polyurethane as a reactive flame retardant. Synthesis is made to form DOPO-MBAP with synergistic nitrogen and phosphorus with excellent flame retardant properties.

Benefits of technology

This flame retardant has better stability in polyurethane, is not easy to migrate, and has a long-lasting flame retardant performance, which significantly improves the flame retardant performance of water-based polyurethane and reaches the V-0 level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932511900000021
    Figure BDA0004932511900000021
  • Figure BDA0004932511900000022
    Figure BDA0004932511900000022
  • Figure BDA0004932511900000071
    Figure BDA0004932511900000071
Patent Text Reader

Abstract

The invention relates to the field of polyurethane, and discloses a DOPO phosphamide derivative flame retardant, a preparation method thereof and application of the DOPO phosphamide derivative flame retardant in waterborne polyurethane. According to the preparation method, p-aminophenol is taken as a nitrogen component and is subjected to a binding reaction with benzoyl chloride, a double-terminal hydroxyl structure is introduced, and then the DOPO phosphamide derivative is prepared through a DOPO reaction. The DOPO phosphamide derivative has the characteristics of no halogen, no smoke, no toxicity and lasting flame retardant property; meanwhile, the flame retardant can be used as a reactive flame retardant to participate in a synthetic reaction of waterborne polyurethane, so that the flame retardant has better stability in polyurethane and is not easy to migrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyurethane, and in particular to a DOPO phosphoramide derivative flame retardant and a preparation method thereof and application thereof in waterborne polyurethane. Background Art

[0002] As an important polymer material, polyurethane (PU) is widely used in many fields such as home appliances, automobiles, construction, furniture, and footwear due to its excellent physical and mechanical properties, wear resistance, oil resistance, chemical resistance, ozone resistance, electrical insulation, and good processing performance. However, the flammability of polyurethane is a major hidden danger in its application process. Especially under high temperature or fire conditions, polyurethane materials will burn rapidly and release a large amount of toxic gases, posing a great threat to personnel safety and the environment.

[0003] 9,10-Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) is a typical phosphorus-containing flame retardant. The biphenyl ring and phenanthrene ring structure in the DOPO molecular structure, especially the phosphorus element in the form of a cyclic O=PO bond, make it have higher chemical stability and thermal stability. More importantly, DOPO has better flame retardant properties than general non-cyclic organic phosphates.

[0004] At present, there are few examples of using DOPO as a base material to prepare DOPO phosphoramide derivative flame retardants, especially no reports on their application in waterborne polyurethane. Therefore, it is of great significance to study the preparation of DOPO phosphoramide derivative flame retardants that can be used in waterborne polyurethane. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a DOPO phosphoramide derivative flame retardant and a preparation method thereof and application in waterborne polyurethane. The present invention uses p-aminophenol as a nitrogen component, introduces a double-terminal hydroxyl structure by combining with benzoyl chloride, and then prepares a DOPO phosphoramide derivative through a DOPO reaction. The DOPO phosphoramide derivative has the characteristics of being halogen-free, smokeless, non-toxic, and having a long-lasting flame retardant performance; at the same time, it can be used as a reactive flame retardant to participate in the synthesis reaction of waterborne polyurethane, so it has better stability in polyurethane and is not easy to migrate.

[0006] The specific technical scheme of the present invention is:

[0007] First, the present invention provides a DOPO phosphoramide derivative flame retardant, the chemical structure of which is as follows:

[0008]

[0009] The present invention uses p-aminophenol as a nitrogen component, introduces a double-terminal hydroxyl structure through a reaction with benzoyl chloride, and then prepares a DOPO phosphoramide derivative through a DOPO reaction. The DOPO phosphoramide derivative is a new type of nitrogen-phosphorus flame retardant. The p-aminophenol has an aniline structure, and the N connected to the benzene ring has a stronger flame retardant property, which has better performance than alkylamines. However, the flame retardant effect of nitrogen-based flame retardants used alone is poor. To this end, the present invention prepares a DOPO phosphoramide derivative flame retardant (DOPO-MBAP) containing both nitrogen and phosphorus through a series of reactions. The synergistic flame retardant performance brought about by the direct connection of PN elements in the flame retardant is better than the performance of PN elements not connected. In addition, it can be used as a reactive flame retardant to participate in the synthesis reaction of waterborne polyurethane, so it has better stability in polyurethane. The composite flame retardant is halogen-free, smoke-free, non-toxic, non-migrating, and has a long-lasting flame retardant performance.

[0010] Secondly, the present invention provides a method for preparing the above-mentioned DOPO phosphoramide derivative flame retardant, comprising the following steps:

[0011] Step 1: using p-aminophenol and methoxybenzoyl chloride as raw materials, and obtaining methoxybenzamide p-phenol (MBAP) after reaction;

[0012] Step 2: using methoxybenzamide p-phenol as a raw material, reacting in the presence of AlCl3 and anhydrous ethanethiol, and extracting with dichloromethane to obtain a methoxybenzamide p-phenol demethoxy intermediate;

[0013] Step 3: Using the demethoxylated intermediate of phenol by methoxybenzamide and DOPO as raw materials, a DOPO phosphoramide derivative flame retardant (DOPO-MBAP) is obtained after reaction.

[0014] The synthetic route of the present invention is as follows:

[0015]

[0016] Preferably, the above preparation method specifically comprises:

[0017] Step 1: Add ethyl acetate dissolved with 4-6 ml of triethylamine and 2-4 g of p-aminophenol into a reaction container, add 4-6 ml of methoxybenzoyl chloride at 0-5° C., stir to react, filter the crude product, wash it, and vacuum dry it to obtain methoxybenzamide p-phenol (MBAP);

[0018] Step 2: Add methoxybenzamide p-phenol to dichloromethane dissolved with 30-50 mg AlCl3 and 1-3 ml anhydrous ethanethiol, stir and react at 0-5°C, extract the reaction mixture with dichloromethane, take the organic layer, and vacuum dry to obtain a demethoxy intermediate of methoxybenzamide p-phenol;

[0019] Step 3: adding dichloromethane containing triethylamine dissolved in carbon tetrachloride at 1-10°C, controlling the temperature at 10-15°C, adding methoxybenzamide to phenol demethoxy intermediate and DOPO, raising the temperature to 20-30°C and stirring for reaction; filtering the product and evaporating the filtrate under reduced pressure, washing with ethanol, and vacuum drying to obtain a DOPO phosphoramide derivative flame retardant (DOPO-MBAP); the amount of DOPO used is 1-1.3 times the amount used for the reaction of methoxybenzamide to phenol demethoxy intermediate.

[0020] Preferably, in step 1: the amount of ethyl acetate used is 30-50 ml.

[0021] Preferably, in step 2: the amount of dichloromethane used is 10-30 ml, and dichloromethane serves as a co-solvent and also as an extractant.

[0022] Preferably, in step 2: the reaction time of the stirring reaction is 2-3h.

[0023] Preferably, in step 3: the amount of carbon tetrachloride used is 2-3 ml, the amount of triethylamine used is 2-4 ml, and the amount of dichloromethane used is 20-30 mL.

[0024] Preferably, in step 3: the vacuum drying conditions are: 70-90° C., 1-3 h.

[0025] Finally, the present invention provides an application of the above-mentioned DOPO phosphoramide derivative flame retardant in the preparation of waterborne polyurethane, comprising: dissolving isophorone diisocyanate, polypropylene alcohol, and a catalyst in acetone, stirring and reacting at 80-90°C for 0.5-1.5h, adding the DOPO phosphoramide derivative flame retardant, stirring and reacting for 0.5-1.5h, cooling to 65-75°C, adding 2,2-dihydroxymethylpropionic acid, stirring for 0.5-1.5h, then cooling to 35-45°C, adding triethylamine, stirring and reacting for 0.5-1.5h, cooling to room temperature, adding water, stirring and emulsifying for 20-40min, and obtaining an emulsion containing waterborne polyurethane.

[0026] Preferably, the amount of isophorone diisocyanate is 5-8 g, the amount of polypropylene alcohol is 20-50 g, the amount of 2,2-hydroxymethylpropionic acid is 0.5-2 g, and the amount of DOPO phosphoramide derivative flame retardant is 0.2-2 g.

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] The invention uses p-aminophenol as a nitrogen component, introduces a double-terminal hydroxyl structure by combining with benzoyl chloride, and then prepares a DOPO phosphoramide derivative by DOPO reaction. The DOPO phosphoramide derivative has the characteristics of being halogen-free, smoke-free, non-toxic, and having a long-lasting flame retardant performance; at the same time, it can be used as a reactive flame retardant to participate in the synthesis reaction of waterborne polyurethane, so it has better stability in polyurethane and is not easy to migrate. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the embodiments.

[0030] Example 1

[0031] 1) Preparation of methoxybenzamide p-phenol (MBAP): In a round-bottom flask, add a mixture of 3.5 ml of dichloromethane and 3.27 g (0.03 mol) of p-aminophenol dissolved in 30 ml of dichloromethane, slowly dropwise add a mixed solution of 4.06 ml (0.03 mol) of methoxybenzoyl chloride dissolved in 10 ml of dichloromethane at about 0°C under ice bath conditions, and add dichloromethane solvent in time. Filter the crude product, wash several times, and vacuum dry to obtain a white powder.

[0032] 2) Preparation of the intermediate of demethoxylation of phenol by methoxybenzamide: 1 g of the powder obtained in step 1 was added to 20 ml of dichloromethane solution containing 0.75 g (1.4 equivalents) of AlCl3, and stirred at 0°C for 2.5 h. After stirring, the reaction was quenched with dilute hydrochloric acid, and vacuum filtered and dried to obtain the intermediate product.

[0033] 3) Preparation of DOPO-MBAP: Control the temperature below 15°C, add a mixture of 2.3g of methoxybenzamide demethoxylated intermediate of phenol and 1 equivalent of DOPO to 50ml of dichloromethane, and add a dichloromethane solution of 40ml of triethylamine dissolved in 0.8ml of carbon tetrachloride at 5°C. Then warm to room temperature and stir overnight. Filter the product and evaporate the filtrate under reduced pressure, wash with saturated sodium bicarbonate, deionized water, acetone, and ethanol for multiple times, and finally dry under vacuum at 80°C for 2h to obtain the final product DOPO-MBAP.

[0034] 5) Preparation of DOPO-MBAP waterborne polyurethane: Weigh 6.968g (0.031mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 0.397g of DOPO-MBAP and dissolve them in 50ml of acetone. Stir and react at 85°C for 2h, then add 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid and lower the temperature to 70°C and stir for 1h. Then cool to 40°C, add 1.39ml (0.01mol) of triethylamine and pay attention to the viscosity of the system. Add acetone in time and stir for 1h. Cool to room temperature, add 100ml of deionized water, emulsify for 0.5h under high-speed stirring to obtain waterborne polyurethane emulsion WPU / 1% DOPO-MBAP.

[0035] Example 2

[0036] 1) The preparation of DOPO-MBAP is the same as in Example 1.

[0037] 2) Preparation of DOPO-MBAP waterborne polyurethane: 8.279g (0.037mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 2.139g of DOPO-MBAP were weighed and dissolved in 50ml of acetone. After stirring at 85°C for 2h, 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid was added and the temperature was lowered to 70°C and stirred for 1h. Then the temperature was lowered to 40°C, 1.39ml (0.01mol) of triethylamine was added, and attention was paid to the viscosity of the system. Acetone was added in time and stirred for 1h. The temperature was lowered to room temperature, 100ml of deionized water was added, and emulsification was carried out under high-speed stirring for 0.5h to obtain a waterborne polyurethane emulsion WPU / 5% DOPO-MBAP.

[0038] Example 3

[0039] 1) The preparation of DOPO-MBAP is the same as in Example 1.

[0040] 2) Preparation of DOPO-MBAP waterborne polyurethane: Weigh 10.230g (0.046mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 4.74g of DOPO-MBAP and dissolve them in 50ml of acetone. Stir and react at 85°C for 2h, then add 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid and lower the temperature to 70°C and stir for 1h. Then cool to 40°C, add 1.39ml (0.01mol) of triethylamine and pay attention to the viscosity of the system. Add acetone in time and stir for 1h. Cool to room temperature, add 100ml of deionized water, emulsify for 0.5h under high-speed stirring to obtain waterborne polyurethane emulsion WPU / 10% DOPO-MBAP.

[0041] Example 4

[0042] 1) The preparation of DOPO-MBAP is the same as in Example 1.

[0043] 2) Preparation of DOPO-MBAP waterborne polyurethane: Weigh 12.644g (0.057mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 7.94g of DOPO-MBAP and dissolve them in 50ml of acetone. Stir and react at 85°C for 2h, then add 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid and lower the temperature to 70°C and stir for 1h. Then cool to 40°C, add 1.39ml (0.01mol) of triethylamine and pay attention to the viscosity of the system. Add acetone in time and stir for 1h. Cool to room temperature, add 100ml of deionized water, emulsify for 0.5h under high-speed stirring to obtain waterborne polyurethane emulsion WPU / 10% DOPO-MBAP.

[0044] Comparative Example 1

[0045] Preparation of nitrogen-phosphorus flame retardant-free waterborne polyurethane: Weigh 6.283 ml (0.03 mol) of isophorone diisocyanate, 30 g (0.01 mol) of polypropylene glycol, and three drops of dibutyltin dilaurate, dissolve in 50 ml of acetone, stir and react at 85 ° C for 2 hours, then add 1.34 g (0.01 mol) of 2,2-dihydroxymethyl propionic acid and lower the temperature to 70 ° C, stir for 1 hour. Then cool to 40 ° C, add 1.39 ml (0.01 mol) of triethylamine, pay attention to the viscosity of the system, add acetone in time, stir and react for 1 hour. Then cool to room temperature, add 100 ml of deionized water, emulsify for 0.5 hours under high-speed stirring, and obtain waterborne polyurethane emulsion WPU.

[0046] Comparative Example 2

[0047] Preparation of nitrogen-containing flame retardant waterborne polyurethane: 9.905g (0.045mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 2.224g of MBAP (prepared according to step 1 of Example 1) were weighed and dissolved in 50ml of acetone. After stirring and reacting at 85°C for 2h, 1.34g (0.01mol) of 2,2-dimethylolpropionic acid was added and the temperature was lowered to 70°C and stirred for 1h. Then the temperature was lowered to 40°C, 1.39ml (0.01mol) of triethylamine was added, and attention was paid to the viscosity of the system. Acetone was added in time and stirred for 1h. The temperature was lowered to room temperature, 100ml of deionized water was added, and emulsified for 0.5h under high-speed stirring to obtain a waterborne polyurethane emulsion WPU / 5% MBAP.

[0048] Comparative Example 3

[0049] Preparation of nitrogen-containing flame retardant waterborne polyurethane: Weigh 14.149g (0.063mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, three drops of dibutyltin dilaurate and 2.447g of p-aminophenol and dissolve them in 50ml of acetone. Stir and react at 85°C for 2h, then add 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid and lower the temperature to 70°C, stirring for 1h. Then cool to 40°C, add 1.39ml (0.01mol) of triethylamine, pay attention to the viscosity of the system, add acetone in time, and stir and react for 1h. Then cool to room temperature, add 100ml of deionized water, emulsify for 0.5h under high-speed stirring to obtain waterborne polyurethane emulsion WPU / 5%AP.

[0050] Comparative Example 4

[0051] Preparation of waterborne polyurethane containing phosphorus flame retardant: Weigh 6.283ml (0.03mol) of isophorone diisocyanate, 30g (0.01mol) of polypropylene glycol, and three drops of dibutyltin dilaurate and dissolve them in 50ml of acetone. Stir and react at 85°C for 2h, then add 1.34g (0.01mol) of 2,2-dihydroxymethylpropionic acid and lower the temperature to 70°C, and stir for 1h. Then cool to 40°C, add 1.39ml (0.01mol) of triethylamine, pay attention to the viscosity of the system, add acetone in time, and stir and react for 1h. Then cool to room temperature, add 1.951g of DOPO dissolved in 10ml of acetone, add 100ml of deionized water, and emulsify for 0.5h under high-speed stirring to obtain waterborne polyurethane emulsion WPU / 5% DOPO.

[0052] Performance Testing

[0053] The performance of the products obtained in each embodiment and comparative example was tested, and the results are shown in the following table:

[0054]

[0055] As can be seen from the above table, the flame retardant properties of waterborne polyurethane are significantly improved after adding the DOPO-MBAP flame retardant of the present invention, reaching the level of V-0 on 10% DOPO-MBAP, while comparative examples 1, 2, and 3 do not have obvious flame retardant performance improvement. The reason is that MBAP and AP only introduce aniline structure, and this structure alone is not an excellent flame retardant, and cannot greatly increase the nitrogen content of polyurethane, so the flame retardant performance of polyurethane is not greatly improved. The waterborne polyurethane mixed with DOPO has higher chemical stability and thermal stability because of the biphenyl ring and phenanthrene ring structure in the DOPO molecular structure, especially the phosphorus element in the form of a cyclic O=PO bond, which can improve the flame retardant performance to a certain extent. After being synthesized into DOPO-MBAP, there are more PN bonds. The synergistic effect brought by the direct connection of nitrogen and phosphorus elements improves their respective flame retardant properties, and DOPO-MBAP greatly increases the nitrogen and phosphorus components in polyurethane, effectively improving the flame retardant properties of waterborne polyurethane.

[0056] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0057] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A DOPO phosphoramide derivative flame retardant, characterized in that: The chemical structure is as follows:

2. A method for preparing the DOPO phosphoramide derivative flame retardant according to claim 1, characterized in that The following steps are involved: Step 1: using p-aminophenol and methoxybenzoyl chloride as raw materials, and obtaining methoxybenzamide p-phenol after reaction; Step 2: using methoxybenzamide p-phenol as a raw material, reacting in the presence of AlCl3 and anhydrous ethanethiol, and extracting with dichloromethane to obtain a methoxybenzamide p-phenol demethoxy intermediate; Step 3: Using methoxybenzamide as the demethoxylated intermediate of phenol and DOPO as raw materials, a DOPO phosphoramide derivative flame retardant is obtained after reaction.

3. The preparation method according to claim 2, characterized in that Specifically include: Step 1: Add ethyl acetate dissolved with 4-6 ml of triethylamine and 2-4 g of p-aminophenol into a reaction container, add 4-6 ml of methoxybenzoyl chloride at 0-5° C., stir to react, filter the crude product, wash it, and vacuum dry it to obtain methoxybenzamide p-phenol; Step 2: Add methoxybenzamide p-phenol to dichloromethane dissolved with 30-50 mg AlCl3 and 1-3 ml anhydrous ethanethiol, stir and react at 0-5°C, extract the reaction mixture with dichloromethane, take the organic layer, and vacuum dry to obtain a demethoxy intermediate of methoxybenzamide p-phenol; Step 3: adding dichloromethane containing triethylamine dissolved in carbon tetrachloride at 1-10°C, controlling the temperature at 10-15°C, adding methoxybenzamide to phenol demethoxy intermediate and DOPO, raising the temperature to 20-30°C and stirring for reaction; filtering the product and evaporating the filtrate under reduced pressure, washing with ethanol, and vacuum drying to obtain a DOPO phosphoramide derivative flame retardant; the amount of DOPO used is 1-1.3 times the amount used for the reaction of methoxybenzamide to phenol demethoxy intermediate.

4. The preparation method according to claim 3, characterized in that: In step 1: the amount of ethyl acetate used is 30-50 ml.

5. The preparation method according to claim 3, characterized in that: In step 2: the amount of dichloromethane used is 10-30 ml.

6. The preparation method according to claim 3, characterized in that: In step 2: the reaction time of the stirring reaction is 2-3h.

7. The preparation method according to claim 3, characterized in that: In step 3: the amount of carbon tetrachloride is 2-3 ml, the amount of triethylamine is 2-4 ml, and the amount of dichloromethane is 20-30 ml.

8. The preparation method according to claim 3, characterized in that: In step 3: the vacuum drying conditions are: 70-90°C, 1-3h.

9. Use of the DOPO phosphoramide derivative flame retardant according to claim 1 or the DOPO phosphoramide derivative flame retardant obtained by the preparation method according to any one of claims 2 to 8 in the preparation of waterborne polyurethane, characterized in that include: Dissolve isophorone diisocyanate, polypropylene glycol and a catalyst in acetone, stir and react at 80-90°C, add a DOPO phosphoramide derivative flame retardant, stir and react, cool to 65-75°C, add 2,2-dihydroxymethylpropionic acid, stir, then cool to 35-45°C, add triethylamine, stir and react, cool to room temperature, add water, stir and emulsify to obtain an emulsion containing waterborne polyurethane.

10. The use according to claim 9, characterized in that: The dosage of the isophorone diisocyanate is 5-8 g, the dosage of the polypropylene alcohol is 20-50 g, the dosage of the 2,2-hydroxymethyl propionic acid is 0.5-2 g, and the dosage of the DOPO phosphoramide derivative flame retardant is 0.2-2 g.

Citation Information

Patent Citations

  • Halogen-free reaction type flame retardant for polyurethane foam as well as preparation method and application thereof

    CN103694434A

  • DOPO-based flame retardant, and preparation method thereof

    CN106243385A

  • Waterborne polyurethane fabric finishing agent with flame-retardant and antifouling functions and preparation method thereof

    CN111270525A

  • Phosphamide-containing DOPO derivative and preparation method and application thereof

    CN115651025A

  • Flame-retardant and ultraviolet-shielding waterborne polyurethane and preparation method thereof

    CN115960331A

Cited By

  • Washable weather-resistant flame-retardant waterborne polyurethane finishing agent as well as preparation method and application thereof

    CN122082253A