Delayed tackifying polymer emulsion and preparation method thereof
By introducing dynamic covalent bonds of borate ester into polymers, forming a crosslinked structure and slowly breaking bonds in the formation, the problem of polymer viscosity reduction in shear and formation is solved, the delayed viscosity increase effect is achieved, and the oil field is improved Recovery rate.
Patent Information
- Application Number
- CN202411012191.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The molecular chain breaks during pumping and shearing of existing polymers, resulting in a decrease in the viscosity of the aqueous phase, which cannot effectively improve the recovery rate, and the concentration decreases due to formation adsorption, which cannot achieve the expected viscosity-enhancing effect.
The polymer with dynamic covalent bonds of borate ester is synthesized under alkaline conditions. After entering the formation, the bonds are slowly broken under neutral conditions and gradually become linear structures to achieve delayed tackification.
The viscosity of the polymer solution in high-temperature brine gradually increases, extending the time to reach the maximum viscosity, significantly improving the recovery rate and avoiding the problems of molecular chain breakage and concentration drop.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a delayed viscosity-increasing polymer emulsion and a preparation method thereof, belonging to the technical field of enhancing crude oil recovery. Background Art
[0002] Polymer flooding is an important method for improving oil recovery in oil fields. Its main principle is to increase the viscosity of the water phase, reduce the oil-water mobility ratio, and thus expand the sweep factor to improve the recovery rate. In order to maximize the viscosity of the water phase, the molecular weight of the polymer flooding polymer is usually large. However, after the high molecular weight polymer is sheared in the pumping, pipeline and near-well area, the molecular chain breaks and the molecular weight drops significantly, thus failing to achieve the expected effect. In addition, due to the adsorption of the formation to the polymer, the concentration of the polymer usually drops significantly when it reaches the deep formation, and the viscosity-increasing effect does not meet expectations. If there is a polymer with a delayed viscosity-increasing effect, that is, the molecular chain is curled during injection, the polymer solution has basically no viscosity (thereby ensuring that the chain will not break due to strong shearing), and the molecular chain slowly stretches after entering the formation, and viscosity is increased in the deep formation, it can effectively solve the above problems. Summary of the invention
[0003] The purpose of the present invention is to provide a delayed viscosity increasing polymer emulsion. The present invention introduces borate dynamic covalent bonds for the first time into the preparation of a polymer with delayed viscosity increasing properties. The polymer is synthesized under alkaline conditions and contains a plurality of borate groups therein to give the polymer a cross-linked structure (the solution has no viscosity). After the polymer solution enters the formation, the borate bonds are slowly broken under neutral conditions, and the polymer gradually changes into a linear structure, thereby achieving a slow viscosity increasing effect.
[0004] The method for preparing the delayed viscosity-increasing polymer emulsion provided by the present invention comprises the following steps:
[0005] S1, dissolving acrylamide, acrylic acid, 3-allyloxy-1,2-propylene glycol and a diboric acid compound in water, and adjusting the pH value to 8.5-9.5 to obtain an aqueous phase; dissolving a composite surfactant in white oil to form an oil phase, and adding the aqueous phase to the oil phase under shear emulsification conditions, and shear emulsifying to form a high internal phase oil-in-water emulsion;
[0006] S2, lowering the temperature of the high internal phase oil-in-water emulsion, passing nitrogen to remove oxygen, and then adding an initiator to carry out polymerization reaction to obtain the product.
[0007] The synthetic route of the preparation method of the present invention is as follows:
[0008]
[0009] In the above-mentioned preparation method, in step S1, the total mass ratio of the acrylamide to the acrylic acid and the 3-allyloxy-1,2-propanediol is 3.5 to 5:1;
[0010] The mass ratio of the acrylic acid to the 3-allyloxy-1,2-propanediol is 15:1 to 25:1, preferably 15:1, 20:1 or 25:1.
[0011] In the above preparation method, in step S1, the diboric acid compound is a product of the reaction of triethylenetetramine and 2-formylphenylboric acid in a molar ratio of 1:2.
[0012] In the above preparation method, in step S1, the molar ratio of the diboric acid compound to the 3-allyloxy-1,2-propanediol is 1:1.
[0013] In the above preparation method, in step S1, the total mass concentration of monomers in the aqueous phase is 40-50%, such as 40% or 50%;
[0014] The monomers include the acrylamide, the acrylic acid, the 3-allyloxy-1,2-propanediol and the diboric acid compound.
[0015] In the above preparation method, in step S1, the composite surfactant is a composite of Span80 and T81, and the mass ratio of the two is 7 to 9:1;
[0016] The viscosity of the high internal phase oil-in-water emulsion in step S1 is greater than 300 cp.
[0017] In the above preparation method, in step S2, the initiator is ammonium persulfate and sodium bisulfite;
[0018] The mass ratio of the sodium bisulfite to the ammonium persulfate is 1.2 to 6:1;
[0019] The amount of ammonium persulfate added is 0.05% to 0.1% of the total monomer mass, preferably 0.05%, 0.075% or 0.1%.
[0020] The viscosity of the delayed viscosity-increasing polymer emulsion provided by the present invention in saline with a temperature of ≥50°C gradually increases with time; its viscosity in saline with a temperature of ≥50°C gradually increases with the extension of the storage time, and usually reaches the maximum within 5 to 15 days.
[0021] Compared with the existing common oil displacement polymers, the technical effects of the present invention are:
[0022] After the delayed viscosity-increasing polymer emulsion of the present invention is dissolved in water, its viscosity does not reach the maximum very quickly, but increases slowly with time. DETAILED DESCRIPTION
[0023] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0024] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0025] Embodiment 1,
[0026] S1) Add 60g acrylamide, 14.06g acrylic acid, and 72.17g deionized water to a 250mL beaker, add sodium hydroxide to adjust the solution pH to 9 under ice bath and stirring, and then add 0.94g 3-allyloxy-1,2-propanediol and 2.83 g of diboronic acid compound (synthesized according to the experimental method in the literature “Ding Xiaoya, Wang Yu, Li Gao, Xiao Chunsheng, Chen Xuesi. Injectable self-healing hydrogel based on imine borate and borate ester bonds and its multi-responsive properties. Journal of Polymer Science, 2019, 50(5): 505-514”) were stirred and completely dissolved to obtain an aqueous phase; 4 g of emulsifier Span80, 0.45 g of emulsifier T-81 and 45.45 g of white oil were added to a 250 mL beaker and completely dissolved to obtain an oil phase; the oil phase and the aqueous phase were poured into a shear emulsifier, and the shear emulsifier was turned on (12000 rpm) for shearing for 8-9 min. When the viscosity of the emulsion was greater than 300 cp, a high internal phase oil-in-water emulsion was obtained.
[0027] S2) The high internal phase oil-in-water emulsion was poured into a 500 mL three-necked flask, cooled to 15° C., deoxygenated with nitrogen for 15 min, and then 0.0375 g of ammonium persulfate and 0.0562 g of sodium bisulfite were added. After exothermic polymerization for 4 h, a delayed viscosity-increasing polymer emulsion was obtained.
[0028] Comparative Example 1
[0029] The basic implementation of this embodiment is the same as that of embodiment 1, except that in this embodiment, 66 g of acrylamide, 15.47 g of acrylic acid, 1.03 g of 3-allyloxy-1,2-propylene glycol, 3.10 g of diboric acid compound, and 64.4 g of deionized water are added to S1. In S2, 0.0412 g of ammonium persulfate and 0.0618 g of sodium bisulfite are added.
[0030] Embodiment 2,
[0031] The basic implementation of this embodiment is the same as that of embodiment 1, except that in this embodiment, 48 g of acrylamide, 11.25 g of acrylic acid, 0.75 g of 3-allyloxy-1,2-propylene glycol, 2.25 g of diboric acid compound, and 87.75 g of deionized water are added to S1. In S2, 0.03 g of ammonium persulfate and 0.045 g of sodium bisulfite are added.
[0032] Embodiment 3,
[0033] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 14.28 g of acrylic acid, 0.72 g of 3-allyloxy-1,2-propylene glycol, 2.16 g of a dibasic boric acid compound, and 72.84 g of deionized water are added to S1.
[0034] Embodiment 4,
[0035] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 14.42 g of acrylic acid, 0.58 g of 3-allyloxy-1,2-propylene glycol, 1.74 g of a dibasic boric acid compound, and 73.26 g of deionized water are added to S1.
[0036] Comparative Example 2
[0037] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 14.52 g of acrylic acid, 0.48 g of 3-allyloxy-1,2-propylene glycol, 1.44 g of a dibasic boric acid compound, and 73.56 g of deionized water are added to S1.
[0038] Embodiment 5,
[0039] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 0.0562 g of ammonium persulfate and 0.0843 g of sodium bisulfite are added to S2.
[0040] Embodiment 6,
[0041] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 0.075 g of ammonium persulfate and 0.1125 g of sodium bisulfite are added to S2.
[0042] Comparative Example 3
[0043] The basic implementation of this embodiment is the same as that of Embodiment 1, except that in this embodiment, 0.09 g of ammonium persulfate and 0.135 g of sodium bisulfite are added to S2.
[0044] In order to further illustrate the technical effects of the present invention, the present invention also provides relevant tests of the above-mentioned embodiments in practical applications.
[0045] 1. Effect of monomer ratio on delayed viscosity increasing effect of polymer
[0046] A 2000 ppm polymerization product solution was prepared using 1% NaCl saline as solvent. The dissolved oxygen in the solution was removed by vacuum in a glove box and then placed in a vial and sealed. The vial was then placed in an oven at 75° C. for different heat preservation times and the apparent viscosity was measured.
[0047] It can be seen from Table 1 that when the mass ratio of acrylic acid to 3-allyloxy-1,2-propylene glycol is in the range of 15:1 to 25:1, the polymer solution has an obvious delayed viscosity increase phenomenon, and the polymer reaches a maximum viscosity at 10 days. This is because the borate bonds contained in the polymer will slowly hydrolyze when the pH is less than 9, and the cross-linked polymer will slowly become a linear polymer, and the viscosity will slowly increase. When the ratio of the two is 30:1, the polymer has no delayed viscosity increase phenomenon, and its viscosity reaches a maximum in 4 hours. This is because the polymer does not have a cross-linked structure at this time.
[0048] Table 1 Apparent viscosity of the polymerization product solution at different monomer ratios
[0049]
[0050] 2. Effect of monomer concentration on polymerization results
[0051] The effect of monomer concentration on the polymerization results is examined by whether explosive polymerization will occur during the polymerization reaction and whether the products after polymerization will be stratified.
[0052] As shown in Table 2, when the monomer concentration in water is greater than 50%, implosion will occur. This is because when the monomer concentration is too high, the reaction releases more heat, the system dissipates heat slowly, the system temperature rises rapidly, and the reaction speed becomes faster and faster, resulting in implosion. When the monomer concentration is 40-50%, the polymerization product is stable.
[0053] Table 2 Polymerization results at different monomer concentrations
[0054]
[0055] 3. Effect of initiator dosage on polymerization results
[0056] The effect of the amount of initiator added on the polymerization results was investigated by determining whether explosive polymerization would occur during the polymerization reaction and whether the products would be stratified after polymerization.
[0057] As shown in Table 3, when the amount of ammonium persulfate added is greater than 0.1%, implosion occurs. This is because when the amount of initiator added is too large, the number of primary free radicals generated increases, the reaction rate is too fast, and implosion occurs. When the amount of ammonium persulfate added is within the range of 0.05% to 0.1%, the polymerization is stable and the reaction product is stable.
[0058] Table 3 Polymerization results when different initiator addition amounts are used
[0059]
[0060] 4. Effect of temperature on delayed viscosity increase behavior of polymers
[0061] A 2000 ppm polymerization product solution was prepared using 1% NaCl saline as solvent. The dissolved oxygen in the solution was removed by vacuum in a glove box and then placed in a vial and sealed. The apparent viscosity was then measured after being kept at different temperatures for different periods of time.
[0062] As shown in Table 4, when the temperature is 50°C, the polymer viscosity reaches the maximum on the 15th day, when the temperature is 75°C, the polymer viscosity reaches the maximum on the 10th day, and when the temperature is 90°C, the polymer viscosity reaches the maximum on the 5th day. The higher the temperature, the faster the boric acid ester bond contained in the polymer hydrolyzes, and the polymer can change from a cross-linked structure to a linear structure more quickly.
[0063] Table 4 Apparent viscosity of the polymer solution at different storage temperatures
[0064]
[0065] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the embodiments of the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a delayed viscosity-increasing polymer emulsion, comprising the following steps: S1, dissolving acrylamide, acrylic acid, 3-allyloxy-1,2-propylene glycol and a diboric acid compound in water, and adjusting the pH value to 8.5-9.5 to obtain an aqueous phase; dissolving a composite surfactant in white oil to form an oil phase, and adding the aqueous phase to the oil phase under shear emulsification conditions, and shear emulsifying to form a high internal phase oil-in-water emulsion; S2, lowering the temperature of the high internal phase oil-in-water emulsion, passing nitrogen to remove oxygen, and then adding an initiator to carry out polymerization reaction to obtain the product.
2. The preparation method according to claim 1, Features: In step S1, the total mass ratio of the acrylamide to the acrylic acid and the 3-allyloxy-1,2-propylene glycol is 3.5-5:1; The mass ratio of the acrylic acid to the 3-allyloxy-1,2-propanediol is 15:1 to 25:
1.
3. The preparation method according to claim 1 or 2, Features: In step S1, the diboric acid compound is a product of the reaction of triethylenetetramine and 2-formylphenylboric acid in a molar ratio of 1:
2.
4. The preparation method according to any one of claims 1 to 3, Features: In step S1, the molar ratio of the diboric acid compound to the 3-allyloxy-1,2-propanediol is 1:
1.
5. The preparation method according to any one of claims 1 to 4, Features: In step S1, the total mass concentration of monomers in the aqueous phase is 40-50%; The monomers include the acrylamide, the acrylic acid, the 3-allyloxy-1,2-propanediol and the diboric acid compound.
6. The preparation method according to any one of claims 1 to 5, Features: In step S1, the composite surfactant is a composite of Span80 and T81, and the mass ratio of the composite surfactant is 7 to 9:1; The viscosity of the high internal phase oil-in-water emulsion in step S1 is greater than 300 cp.
7. The preparation method according to any one of claims 1 to 6, Features: In step S2, the initiator is ammonium persulfate and sodium bisulfite; The mass ratio of the sodium bisulfite to the ammonium persulfate is 1.2 to 6:1; The amount of ammonium persulfate added is 0.05% to 0.1% of the total monomer mass.
8. The delayed viscosity-increasing polymer emulsion prepared by the method according to any one of claims 1 to 7.
9. Use of the delayed viscosity increasing polymer emulsion according to claim 8 in enhancing crude oil recovery; The viscosity of the delayed viscosity-increasing polymer emulsion in saline water with a temperature of ≧50° C. shows a characteristic of gradually increasing over time.