Polyamide and preparation method thereof
Through short high-temperature stage and low-temperature solid-phase polymerization technology, the problem of insufficient molecular weight and mechanical properties of glutarate polyamide is solved, and the preparation of high-performance polyamide is realized, which is suitable for high-end clothing and composite materials.
Patent Information
- Application Number
- CN202411315717.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to effectively improve the molecular weight and mechanical properties of glutarate polyamide (PA65 or PA55), resulting in the failure to fully reflect its performance, and the preparation method is complex and difficult to repeat.
The short-term high-temperature stage and low-temperature solid-phase polymerization technology scheme is adopted to adjust the polymerization conditions, reduce the impact of cyclization reaction on polymerization, and form a uniform prepolymer and a tight crystal structure, thereby improving the relative viscosity and molecular weight of the polyamide.
It has achieved high relative viscosity and high molecular weight polyamide preparation, with excellent mechanical properties and hygroscopic properties, significantly improved tensile strength and water absorption, and is suitable for high-end clothing fabrics and high-performance composite materials.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyamide, and specifically relates to a polyamide and a preparation method thereof. Background Art
[0002] Polyamide (PA), also known as nylon, has good mechanical properties, heat resistance, wear resistance, chemical resistance, self-lubrication, low friction coefficient, certain flame retardancy and easy processing. It has become the most widely used and produced variety among the five major engineering plastics. It is widely used in electronics, construction, food packaging, national defense and military industry, automobiles, medical treatment, machinery, aerospace, petrochemical and other fields, such as nylon 6 (PA6) and nylon 66 (PA66). As members of the polyamide family, polyamide 65 (PA65) and polyamide 55 (PA55) have chemical structures similar to PA66. In theory, they should have excellent mechanical properties similar to PA66 and higher hygroscopicity, and have great application prospects. In addition, an important source of glutaric acid is the by-product of adipic acid production. With the production of millions of tons of adipic acid worldwide, hundreds of thousands of tons of glutaric acid will be produced each year, providing a stable source of raw materials for the industrial production of glutaric acid-based polyamide (PAX5). In recent years, with the continuous breakthroughs and increasing maturity of the biological preparation technology of glutaric acid, the supply of glutaric acid has increased, promoting the development of bio-based PAX5.
[0003] CN108285532A and CN112920401A respectively disclose a method for preparing PA65, but the number average molecular weight of the PA65 prepared does not exceed 20,000 g / mol, and the tensile strength does not exceed 10 MPa. The polymer molecular weight is low and fails to fully reflect the performance that nylon 65 should have. "Synthesis and Characterization of Nylon 65 [D], Zhengzhou University, 2020" discloses a method for preparing PA65. Unfortunately, the relative viscosity of the prepared PA65 does not exceed 2.1, and the tensile strength is only 45 MPa, which is far from the tensile strength of conventional industrial grade PA66 (≥70 MPa). The core reason why these mechanical properties are not as expected is that the molecular weight of the prepared PAX5 is low, which is not enough to exert the performance that the polymer should have.
[0004] CN114213653A points out that under the traditional melt polymerization process, glutarimide groups appear at the ends of the PAX5 polymer chains, which results in the inability to increase the molecular weight. Although the solution of adding dibasic acid monomers multiple times proposed in the article effectively increases the molecular weight of the polymer, the solution is too complicated. The dibasic acid third monomer added in the late stage of gradual polymerization has a small amount of addition, and a small error will cause a large deviation, which will lead to differences in the sequence structure of the polymer molecular chain, poor experimental repeatability, and greatly reduce the industrial value of the preparation method. At the same time, the introduction of non-glutaric acid polyamide structural unit copolymerization destroys the crystallization of PAX5, thereby affecting other properties. In essence, CN114213653A discloses a method for preparing a polyamide copolymer, rather than a method for preparing nylon 65 or nylon 55.
[0005] Therefore, developing a polymerization method that is simple to operate, highly repeatable, and can effectively increase the molecular weight of PAX5 (PA65 or PA55) and exert its potential performance advantages has become a technical problem that needs to be solved urgently and is of great significance. Summary of the invention
[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide a polyamide and a preparation method thereof. The present invention designs a preparation method of polyamide and adopts a technical scheme of a short high temperature stage and low temperature solid phase polymerization, which is not only conducive to the preparation of uniform prepolymers and compact crystal structures, but also effectively reduces the influence of cyclization reaction on polymerization, thereby obtaining polyamide with high relative viscosity (≥2.2) and high molecular weight (Mn≥21000). The polyamide prepared by the preparation method of the present invention has high mechanical properties and hygroscopic properties.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing polyamide, the preparation method comprising the following steps:
[0009] (1) Polymerization stage I: glutaric acid and diamine are dissolved in water to prepare a polyamide salt solution, and a polymerization reaction of stage I is carried out;
[0010] (2) Polymerization stage II: subjecting the reaction system obtained in step (1) to a polymerization reaction in stage II;
[0011] (3) Polymerization stage III: subjecting the reaction system obtained in step (2) to polymerization reaction in stage III;
[0012] (4) Polymerization stage IV: Cooling the reaction system obtained in step (3) to carry out polymerization reaction in stage IV;
[0013] (5) Polymerization stage V: After subjecting the reaction system obtained in step (4) to stage V polymerization reaction, the temperature is lowered;
[0014] (6) Polymerization stage VI: subjecting the reaction system obtained in step (5) to a polymerization reaction in stage VI, and then cooling the reaction system to obtain a polyamide;
[0015] The temperature of the polymerization reaction in the steps (1), (2), (4) to (6) is less than the temperature of the polymerization reaction in the step (3);
[0016] The polymerization reaction temperature in step (3) is 230-270° C. and the time is ≤1h.
[0017] In the prior art, the molecular weight or relative viscosity of PA65 and PA55 is limited. The essence is that the polymerization time is too long at high temperature (≥230°C) or there is a high temperature negative pressure environment. Because the cyclization reaction between the terminal carboxyl group capped with glutaric acid and the adjacent amide group in a high temperature environment competes with the polymerization reaction of molecular chain growth (reaction between the terminal carboxyl group and the terminal amino group), snatching and consuming the limited terminal carboxyl groups, and the higher the temperature, the more intense this competition. In the melt polymerization process, the long-term high temperature environment causes a large number of terminal carboxyl groups to undergo cyclization reactions with adjacent amide groups to form a relatively stable six-membered ring, the molecular chain is capped, and the growth stops. Since both the cyclization reaction and the polymerization reaction require the removal of water, the negative pressure environment is beneficial to the polymerization reaction when the competition between the two is weak, but the negative pressure environment is not conducive to the growth of the molecular chain when the competition between the two is strong.
[0018] In addition, the present invention has found that the hydrogen bond arrangement between the molecular chains of glutaric acid-based polyamide (PA65 and PA55) is slightly different from that of the traditional polyamide PA66, resulting in differences in their crystallization behavior and the crystal structure formed thereafter from PA66. The molecular chains of glutaric acid-based polyamide (PA65 and PA55) crystallize at a relatively low temperature to form a loose crystal structure with a melting point lower than 250°C. For example, for PA65, the melting point of the crystal structure is between 230 and 248°C; while when crystallizing at a relatively high temperature, the polymer molecular chains first crystallize and then melt and recrystallize, forming a relatively compact crystal structure with a melting point higher than 250°C (250 to 260°C), a stronger force between the molecular chains, and a more compact molecular chain, which is conducive to further reaction between the molecular chains and increases the molecular weight of the polymer.
[0019] In view of the above problems, the present invention provides a method for preparing polyamide. The present invention changes the traditional practice of long-term high-temperature polymerization (≥230°C) and high-temperature negative pressure polymerization for polyamide polymerization, and adopts a technical solution of a short high-temperature stage (step (3)) and low-temperature solid phase polymerization (step (4)-step (6)), which is not only conducive to the preparation of uniform prepolymers and compact crystalline structures, but also effectively reduces the influence of cyclization reactions on polymerization, thereby obtaining polyamide with high relative viscosity (≥2.2) and high molecular weight (Mn≥21000). The polyamide prepared by the preparation method of the present invention has high mechanical properties and hygroscopic properties.
[0020] In the present invention, the polymerization reaction temperature in step (3) is 230-270°C (for example, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C or 270°C, etc.), and the time is ≤1h (for example, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min, etc.).
[0021] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0022] As a preferred technical solution of the present invention, the diamine is selected from pentamethylenediamine and / or hexamethylenediamine.
[0023] Preferably, the molar ratio of glutaric acid to diamine is (0.990-1.005):1 (for example, it can be 0.990:1, 0.992:1, 0.994:1, 0.996:1, 0.998:1, 1:1, 1.002:1, 1.004:1 or 1.005:1, etc.), and more preferably 1:1.
[0024] Preferably, the mass concentration of the polyamide salt in the polyamide salt solution is 30-90% (for example, it can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%, etc.), and more preferably 45-75%.
[0025] As a preferred technical solution of the present invention, the temperature of the polymerization reaction in step (1) is 150-190°C, for example, it can be 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C or 190°C, etc.
[0026] Preferably, the polymerization reaction time in step (1) is 0.5 to 6 h (for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h, etc.), more preferably 1 to 3 h.
[0027] Preferably, the polymerization reaction in step (1) is carried out in a closed container under a protective gas atmosphere, and the protective gas comprises an inert gas.
[0028] As a preferred technical solution of the present invention, the temperature of the polymerization reaction in step (2) is 190-230°C, for example, it can be 190°C, 193°C, 196°C, 198°C, 200°C, 202°C, 205°C, 208°C, 208°C, 211°C, 214°C, 217°C, 220°C, 224°C, 227°C or 230°C, etc.
[0029] Preferably, the polymerization reaction time in step (2) is 0.5 to 6 h (for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h, etc.), more preferably 1 to 3 h;
[0030] Preferably, the polymerization reaction pressure in step (2) is 0 to 2.5 MPa, for example, 0 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.3 MPa, 1.5 MPa, 1.7 MPa, 2 MPa, 2.2 MPa, 2.4 MPa or 2.5 MPa.
[0031] As a preferred technical solution of the present invention, the pressure of the polymerization reaction in step (3) is 0 to 2.5 MPa, for example, it can be 0 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.3 MPa, 1.5 MPa, 1.7 MPa, 2 MPa, 2.2 MPa, 2.4 MPa or 2.5 MPa, etc.
[0032] As a preferred technical solution of the present invention, the cooling rate in step (4) is ≥1°C / min (for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or 12°C / min, etc.), and is further preferably 2-10°C / min.
[0033] Preferably, the temperature of the reaction system after cooling is ≤220°C, for example, it may be 200°C, 202°C, 204°C, 206°C, 208°C, 210°C, 212°C, 214°C, 216°C, 218°C or 220°C, etc.
[0034] As a preferred technical solution of the present invention, the temperature of the polymerization reaction in step (5) is 200-220°C, for example, it can be 200°C, 202°C, 204°C, 206°C, 208°C, 210°C, 212°C, 214°C, 216°C, 218°C or 220°C.
[0035] Preferably, the polymerization reaction time in step (5) is 0 to 72 h (for example, 0 h, 6 h, 12 h, 18 h, 24 h, 30 h, 36 h, 42 h, 48 h, 54 h, 60 h, 66 h or 72 h, etc.), more preferably 0 to 24 h.
[0036] Preferably, the temperature of the reaction system after cooling in step (5) is ≤200°C, for example, it can be 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, etc.
[0037] Preferably, the pressure of the polymerization reaction in step (5) is normal pressure or negative pressure.
[0038] As a preferred technical solution of the present invention, the temperature of the polymerization reaction in step (6) is 120-200°C, for example, it can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.
[0039] Preferably, the polymerization reaction time in step (5) is 0 to 360 h (for example, it can be 0 h, 12 h, 40 h, 60 h, 80 h, 100 h, 120 h, 140 h, 160 h, 180 h, 200 h, 240 h, 280 h, 320 h or 360 h, etc.), and more preferably 12 to 120 h;
[0040] Preferably, the temperature of the reaction system after cooling in step (5) is ≤60°C, for example, it can be 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc.
[0041] Preferably, the pressure of the polymerization reaction in step (5) is normal pressure or negative pressure.
[0042] As a preferred technical solution of the present invention, the preparation method of the polyamide specifically comprises the following steps:
[0043] (1) Polymerization stage I: glutaric acid and diamine are dissolved in water to prepare a polyamide salt solution with a mass concentration of 30-90%, and the polymerization reaction is carried out at 150-190° C. in a closed container under a protective gas atmosphere for 0.5-6 hours;
[0044] Wherein, the molar ratio of glutaric acid to diamine is (0.990-1.005):1;
[0045] (2) Polymerization stage II: The reaction system obtained in step (1) is subjected to polymerization reaction at 190-230° C. and 0-2.5 MPa for 0.5-6 h;
[0046] (3) Polymerization stage III: subjecting the reaction system obtained in step (2) to polymerization at 230-270° C. and 0-2.5 MPa for a polymerization time of ≤1 h;
[0047] (4) Polymerization stage IV: cooling the reaction system obtained in step (3) to a temperature of the reaction system ≤ 220° C., with a cooling rate ≥ 1° C. / min;
[0048] (5) Polymerization stage V: at 200-220° C. and normal pressure or negative pressure, the reaction system obtained in step (4) is subjected to polymerization reaction for 0-72 hours, and then the temperature is reduced to a temperature of the reaction system ≤ 200° C.;
[0049] (6) Polymerization stage VI: The reaction system obtained in step (5) is subjected to polymerization reaction at 120-200° C. and normal pressure or negative pressure for 0-360 hours, and then the temperature is reduced to a temperature of the reaction system of ≤60° C. to obtain polyamide.
[0050] It should be noted that in the above-mentioned polyamide preparation method, in steps (1) to (6), the polymerization stage I to the polymerization stage VI can be carried out in the same reactor or in different reactors; at the same time, the pressure increase process, pressure maintenance process and pressure reduction process included in the polymerization stage I to the polymerization stage VI can be completed at one time or divided into multiple processes.
[0051] In a second aspect, the present invention provides a polyamide prepared by the preparation method as described in the first aspect, wherein the relative viscosity of the polyamide is ≥2.2, for example, it can be 2.2, 2.25, 2.32, 2.37, 2.4, 2.45, 2.52, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95 or 3, etc.
[0052] Preferably, the number average molecular weight of the polyamide is ≥21000, for example, it may be 21000, 22000, 23000, 24000, 25000, 26000, 27000, 28000, 29000, 30000, 31000, 32000, 33000, 34000 or 35000, etc.
[0053] Preferably, the polyamide includes any one of polyamide 65, polyamide 55, and a copolymer of polyamide 65 and polyamide 55.
[0054] Compared with the prior art, the present invention has the following beneficial effects:
[0055] (1) High molecular weight polyamide PAX5 (PA65 and PA55) cannot be prepared by conventional melt polymerization methods. However, the present invention designs a method for preparing polyamide and further adopts a technical scheme of a short high temperature stage and low temperature solid phase polymerization to prepare high molecular weight (Mn≥21000) polyamide. At the same time, the preparation method provided by the present invention is simple to operate, has good repeatability, and has very good industrial value.
[0056] (2) The high molecular weight polyamide prepared by the preparation method provided by the present invention can have various advantageous properties of traditional polyamide, such as good heat resistance, wear resistance, chemical resistance and mechanical properties, etc., and its tensile strength is ≥74MPa, elongation at break is ≥4.0%, flexural strength is ≥100MPa, and flexural modulus is ≥2350MPa; at the same time, due to its special intermolecular hydrogen bonding effect, a crystalline structure different from that of PA66 is formed, so that the polyamide has better moisture absorption performance, and its saturated water absorption rate is ≥13.0%, which is nearly three times that of PA66. Therefore, fibers prepared with PAX5 (PA65 and PA55) have better moisture regain and can be used in high-end clothing fabrics with higher added value, and have very good commercial value. In addition, high molecular weight polyamide can also be used as a resin matrix in high-performance fiber-reinforced composites such as glass fiber, carbon fiber and aramid. This composite material has the comprehensive advantages of high performance, easy processing, lightweight, recyclable, low cost, wear resistance and corrosion resistance, breaking through the cost and performance limitations of traditional thermoplastic composites, and is expected to achieve "plastics instead of steel, plastics instead of aluminum, thermoplastics instead of thermosetting" in large scenarios in the fields of transportation logistics, new energy equipment, and architectural decoration.
[0057] (3) Using the preparation method of the present invention, if the selected diamine and diacid are derived from biomass, bio-based polyamide can be prepared. DETAILED DESCRIPTION
[0058] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0059] The sources of some components in the embodiments and comparative examples are as follows:
[0060] Hexamethylenediamine (petroleum-based) comes from Chongqing Huafeng Chemical, glutaric acid (petroleum-based) comes from Liaoyang Hengye Chemical, glutaric acid (bio-based) comes from Yixing Lianyang Chemical, and pentamethylenediamine (bio-based) comes from Cathay Biotechnology.
[0061] It should be noted that the inert atmosphere described in the following examples and comparative examples refers to a nitrogen atmosphere.
[0062] Example 1
[0063] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0064] (1) Polymerization stage I: 24.16 mol of glutaric acid (petroleum-based) and 24.16 mol of hexamethylenediamine were slowly added into water in sequence, and a polyamide salt solution with a concentration of 50 wt% was prepared by continuous stirring. The temperature was raised to 180° C. within 30 minutes under a closed and inert atmosphere, and the reaction was polymerized for 1 hour. The total polymerization time of this stage was 2 hours.
[0065] (2) Polymerization stage II: the temperature was raised to 215°C within 20 minutes, during which the pressure was gradually raised to 1.8 MPa and maintained at 1.8 MPa for 2 hours, accompanied by a slow temperature increase; when the temperature reached 225°C, the pressure was gradually reduced; at the end of this polymerization stage, the temperature was raised to 230°C and the pressure was 1.0 MPa; this polymerization stage lasted for a total of 3 hours;
[0066] (3) Polymerization stage III: the polymerization temperature was raised from 230°C to 245°C within 25 minutes, and the polymerization was carried out at 245°C for 3 minutes, during which the pressure was reduced from 1 MPa to 0 MPa; this stage lasted a total of 28 minutes;
[0067] (4) Polymerization stage IV: the polymer temperature was reduced to 30 °C within 30 min, with an average cooling rate of 7.16 °C / min, and crushed to obtain a granular prepolymer;
[0068] (5) Polymerization stage V: raising the polymerization temperature to 210° C. within 12 hours; polymerizing at 210° C. for 12 hours, and then lowering the temperature to 180° C. within 2 hours;
[0069] (6) Polymerization stage VI: polymerize at 180° C. for 20 hours, and finally reduce the temperature to 30° C. within 12 hours to obtain the polyamide; this polymerization stage maintains a negative pressure of -0.09 MPa.
[0070] Example 2
[0071] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0072] (1) Polymerization stage I: 6.53 mol of glutaric acid (bio-based) and 6.53 mol of hexamethylenediamine were slowly added into water in sequence, and stirred continuously to prepare a polyamide salt solution with a concentration of 70 wt %. The temperature was raised to 175° C. within 25 minutes under a closed and inert atmosphere, and the reaction was polymerized for 25 minutes. The total polymerization time of this stage was 60 minutes.
[0073] (2) Polymerization stage II: the temperature was raised to 210°C within 0.5 hours, during which the pressure was gradually raised to 1.5 MPa and maintained at 1.5 MPa, and the polymerization reaction lasted for 0.5 hours; the temperature was slowly raised to 230°C within 0.5 hours, and the pressure was slowly reduced from 1.5 MPa to 0.5 MPa; this polymerization stage lasted for a total of 1.5 hours;
[0074] (3) Polymerization stage III: the polymerization temperature was raised from 230°C to 250°C within 25 minutes, during which the pressure was reduced from 0.5 MPa to 0 MPa; this stage lasted a total of 25 minutes;
[0075] (4) Polymerization stage IV: The polymer temperature was reduced to 215 °C within 20 min, with an average cooling rate of 1.75 °C / min;
[0076] (5) Polymerization stage V: polymerization at 215°C for 12 hours, pressure of -0.10 MPa; reduced to 30°C within 12 hours;
[0077] (6) Polymerization stage VI: raising the temperature to 190° C. within 12 hours, polymerizing at 190° C. for 84 hours, and the pressure is −0.10 MPa; finally, lowering the temperature to 30° C. within 12 hours to obtain the polyamide.
[0078] Example 3
[0079] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0080] (1) Polymerization stage I: 21.10 mol of glutaric acid (bio-based) and 21.25 mol of pentamethylenediamine were slowly added into water in sequence, and stirred continuously to prepare a polyamide salt solution with a concentration of 45 wt %. The temperature was raised to 170° C. within 30 minutes under a closed and inert atmosphere, and the reaction was polymerized for 1 hour and 30 minutes. The total polymerization time of this stage was 2.5 hours.
[0081] (2) Polymerization stage II: the temperature was raised to 220°C within 1 hour, during which the pressure was gradually raised to 2.0 MPa and maintained at 2.0 MPa, and the polymerization reaction was carried out for 1 hour; the temperature was slowly raised to 230°C within 0.5 hour, and the pressure was slowly reduced from 2.0 MPa to 0.75 MPa; this polymerization stage lasted a total of 2.5 hours;
[0082] (3) Polymerization stage III: the polymerization temperature was raised from 230°C to 243°C within 25 minutes, during which the pressure was reduced from 0.75 MPa to 0 MPa; this stage lasted a total of 25 minutes;
[0083] (4) Polymerization stage IV: The polymer temperature was reduced to 205 °C within 20 min, with an average cooling rate of 2 °C / min;
[0084] (5) Polymerization stage V: polymerization at 205°C for 6 hours, pressure of -0.04 MPa; then reduced to 30°C within 12 hours;
[0085] (6) Polymerization stage VI: raising the temperature to 160° C. within 12 hours, polymerizing at 160° C. for 120 hours; finally lowering the temperature to 30° C. within 12 hours to obtain the polyamide.
[0086] Example 4
[0087] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0088] (1) Polymerization stage I: 25.10 mol of glutaric acid (petroleum-based), 24.00 mol of hexamethylenediamine and 1.00 mol of pentamethylenediamine were slowly added into water in sequence, and stirred continuously to prepare a polyamide salt solution with a concentration of 65 wt %. The temperature was raised to 190° C. within 1 hour under a closed and inert atmosphere, and the reaction was polymerized for 1.5 hours. The total polymerization time of this stage was 3 hours.
[0089] (2) Polymerization stage II: the temperature was raised to 205°C within 15 minutes, during which the pressure was gradually raised to 1.2 MPa and maintained at 1.2 MPa for 1 hour and 45 minutes; the temperature was slowly raised to 230°C within 50 minutes, and the pressure was reduced from 1.2 MPa to 0.35 MPa; the total polymerization time of this stage was 2 hours and 50 minutes;
[0090] (3) Polymerization stage III: The polymerization temperature was raised from 230°C to 242°C within 23 minutes, during which the pressure was reduced from 0.35 MPa to 0.05 MPa; this stage lasted a total of 23 minutes;
[0091] (4) Polymerization stage IV: the polymer temperature is reduced to 35°C within 20 minutes, with an average cooling rate of 10°C / min, and crushed to obtain a granular prepolymer; this polymerization stage takes a total of 20 minutes;
[0092] (5) Polymerization stage V: None
[0093] (6) Polymerization stage VI: raising the polymerization temperature to 150°C within 12 hours; polymerizing at 150°C for 96 hours; finally lowering the temperature to 30°C within 12 hours to obtain the polyamide; the polymerization stage maintained a negative pressure of -0.09 MPa.
[0094] Example 5
[0095] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0096] (1) Polymerization stage I: 100.45 mol of glutaric acid (petroleum-based) and 100.50 mol of hexamethylenediamine were slowly added into water in sequence, and stirred continuously to prepare a polyamide salt solution with a concentration of 75 wt %. The temperature was raised to 185° C. within 1 hour under a closed and inert atmosphere, and the reaction was polymerized for 0.5 hour. The total polymerization time of this stage was 2.5 hours.
[0097] (2) Polymerization stage II: the temperature was raised to 210°C within 20 minutes, during which the pressure was gradually raised to 1.7 MPa and maintained at 1.7 MPa for 1 hour; the temperature was slowly raised to 230°C within 40 minutes, and the pressure was reduced from 1.7 MPa to 0.6 MPa; this polymerization stage lasted a total of 2 hours;
[0098] (3) Polymerization stage III: The polymerization temperature was raised from 230°C to 250°C within 29 minutes, during which the pressure was reduced from 0.6 MPa to 0 MPa; this stage lasted a total of 29 minutes;
[0099] (4) Polymerization stage IV: the polymer temperature was reduced to 30°C within 1 hour, with an average cooling rate of 3.67°C / min, and the polymer was crushed to obtain a granular prepolymer; this polymerization stage lasted for a total of 1 hour;
[0100] (5) Polymerization stage V: the polymerization temperature was raised to 215°C within 12 hours; the polymerization was carried out at 215°C for 3 hours, then the temperature was lowered to 210°C within 2 hours; the polymerization was carried out at 210°C for 3 hours; then the temperature was lowered to 205°C within 2 hours, and the polymerization was carried out at 205°C for 3 hours; finally, the temperature was lowered to 195°C within 2 hours; the negative pressure of -0.10 MPa was maintained during this polymerization stage;
[0101] (6) Polymerization stage VI: polymerize at 195°C for 30 hours; finally, lower the temperature to 30°C within 12 hours to obtain the polyamide; this polymerization stage maintains a negative pressure of -0.10 MPa.
[0102] Example 6
[0103] This embodiment provides a polyamide and a preparation method thereof. The preparation method of the polyamide is as follows:
[0104] (1) Polymerization stage I: 80.39 mol of glutaric acid (petroleum-based) and 80.00 mol of pentamethylenediamine were slowly added into water in sequence, and stirred continuously to prepare a polyamide salt solution with a concentration of 60 wt %. The temperature was raised to 160° C. within 40 minutes under a closed and inert atmosphere, and the reaction was polymerized for 1.5 hours. The total polymerization time of this stage was 3 hours.
[0105] (2) Polymerization stage II: the temperature was raised to 205°C within 30 minutes, during which the pressure was gradually raised to 2.2 MPa and maintained at 2.2 MPa for 30 minutes; the temperature was slowly raised to 230°C within 30 minutes, and the pressure was reduced from 2.2 MPa to 0.9 MPa; this polymerization stage lasted a total of 1 hour and 30 minutes;
[0106] (3) Polymerization stage III: the polymerization temperature was raised from 230°C to 260°C within 35 minutes, during which the pressure was reduced from 0.9 MPa to 0 MPa; this stage lasted a total of 35 minutes;
[0107] (4) Polymerization stage IV: the polymer temperature was reduced to 30°C within 1 hour, with an average cooling rate of 3.83°C / min, and crushed to obtain a granular prepolymer;
[0108] (5) Polymerization stage V: None
[0109] (6) Polymerization stage VI: raising the temperature to 170° C. within 12 hours; polymerizing at 170° C. for 108 hours; finally lowering the temperature to 30° C. within 12 hours to obtain the polyamide; the polymerization stage maintained a negative pressure of -0.09 MPa.
[0110] Comparative Example 1
[0111] This comparative example provides a polyamide and a preparation method thereof, and the preparation method of the polyamide is as follows:
[0112] (1) Polymerization stage I and polymerization stage II are the same as in Example 1;
[0113] (2) Polymerization stage III: the polymerization temperature was raised from 230°C to 250°C within 60 minutes, and the polymerization was carried out at 250°C for 30 minutes, during which the pressure was reduced from 1 MPa to 0 MPa, and then the polymerization was carried out at 250°C under negative pressure for 30 minutes, with a pressure of -0.10 MPa; this stage lasted a total of 120 minutes;
[0114] (3) The polymerization stages IV, V and VI are the same as those in Example 1.
[0115] Comparative Example 2
[0116] This comparative example provides a polyamide and a preparation method thereof, and the preparation method of the polyamide is as follows:
[0117] 24.16 mol of glutaric acid (petroleum-based) and 24.16 mol of hexamethylenediamine were slowly added into water in sequence, and a polyamide salt solution with a concentration of 50 wt% was prepared by continuous stirring. The solution was heated to 230°C within 3 hours under a closed and inert atmosphere, during which the pressure was gradually increased to 1.8 MPa and maintained at 1.8 MPa; the polymerization temperature was then increased from 230°C to 260°C within 60 minutes, and the solution was polymerized at 260°C for 30 minutes, during which the pressure was gradually reduced to 0 MPa; the solution was then polymerized at 260°C under negative pressure for 3 hours at a pressure of -0.10 MPa.
[0118] The properties of the polyamides provided in the above embodiments and comparative examples were tested, and the specific testing methods are as follows: Relative viscosity: measured according to the national standard GB / T12006.1.
[0119] Tensile strength, elongation at break, flexural strength and flexural modulus: tested according to GB / T1040.2-2006 and GB / T9340-2008.
[0120] Saturated water absorption: tested according to GB / T 1034-2008.
[0121] Number average molecular weight: The relative molecular mass of the prepared polyamide was characterized by using an Agilent 1260 Infinity II instrument. Hexafluoroisopropanol was used as a solvent and PMMA was used as a standard sample. A 3 mg / mL solution was prepared and injected into a chromatographic column for testing at 30°C.
[0122] The above performance test results are shown in Table 1 below:
[0123] Table 1
[0124]
[0125]
[0126] It can be seen from the above content that the present invention designs a preparation method for polyamide and further adopts a technical solution of a short high temperature stage and low temperature solid phase polymerization, which is not only conducive to the preparation of uniform prepolymer and compact crystalline structure, but also effectively reduces the influence of cyclization reaction on polymerization, thereby obtaining a polyamide with high relative viscosity and high molecular weight. At the same time, the polyamide prepared by the preparation method of the present invention has high mechanical properties and hygroscopic properties, and its relative viscosity is ≥2.2, specifically 2.30-2.90, the number average molecular weight is ≥21000, specifically 26000-37000, the tensile strength is ≥74MPa, specifically 74.9-82.9MPa, the elongation at break is ≥4.0%, specifically 4.0-5.1%, the flexural strength is ≥100MPa, specifically 101-119MPa, the flexural modulus is ≥2350MPa, specifically 2350-2670MPa, and the saturated water absorption is ≥13.0%, specifically 13.1-14.4%.
[0127] From the comparison between Examples 1-6 and Comparative Example 1, it can be seen that the present invention is designed through the preparation method of polyamide to prepare polyamide with high molecular weight and excellent mechanical properties.
[0128] In summary, the invention designs a method for preparing polyamide and further adopts a technical scheme of a short high-temperature stage and low-temperature solid-phase polymerization, which is not only conducive to the preparation of uniform prepolymers and compact crystalline structures, but also effectively reduces the influence of cyclization reactions on polymerization, thereby obtaining polyamides with high relative viscosity and high molecular weight. At the same time, the polyamide prepared by the preparation method of the present invention has high mechanical properties and hygroscopic properties, and the preparation method is simple to operate, has good repeatability, and has very good industrial value.
[0129] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing polyamide, It is characterized in that The preparation method comprises the following steps: (1) Polymerization stage I: glutaric acid and diamine are dissolved in water to prepare a polyamide salt solution, and a polymerization reaction of stage I is carried out; (2) Polymerization stage II: subjecting the reaction system obtained in step (1) to a polymerization reaction in stage II; (3) Polymerization stage III: subjecting the reaction system obtained in step (2) to polymerization reaction in stage III; (4) Polymerization stage IV: Cooling the reaction system obtained in step (3) to carry out polymerization reaction in stage IV; (5) Polymerization stage V: After subjecting the reaction system obtained in step (4) to stage V polymerization reaction, the temperature is lowered; (6) Polymerization stage VI: subjecting the reaction system obtained in step (5) to a polymerization reaction in stage VI, and then cooling the reaction system to obtain a polyamide; The temperature of the polymerization reaction in the steps (1), (2), (4) to (6) is less than the temperature of the polymerization reaction in the step (3); The polymerization reaction temperature in step (3) is 230-270° C. and the time is ≤1h.
2. The preparation method according to claim 1, It is characterized in that The diamine is selected from pentamethylenediamine and / or hexamethylenediamine; Preferably, the molar ratio of glutaric acid to diamine is (0.990-1.005):1, more preferably 1:1; Preferably, the mass concentration of the polyamide salt in the polyamide salt solution is 30 to 90%, more preferably 45 to 75%.
3. The preparation method according to claim 1, It is characterized in that The polymerization reaction temperature in step (1) is 150-190° C. Preferably, the polymerization reaction time in step (1) is 0.5 to 6 hours, more preferably 1 to 3 hours; Preferably, the polymerization reaction in step (1) is carried out in a closed container under a protective gas atmosphere, and the protective gas comprises an inert gas.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The polymerization reaction temperature in step (2) is 190-230° C. Preferably, the polymerization reaction time in step (2) is 0.5 to 6 hours, more preferably 1 to 3 hours; Preferably, the pressure of the polymerization reaction in step (2) is 0 to 2.5 MPa.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The polymerization reaction pressure in step (3) is 0 to 2.5 MPa.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The cooling rate in step (4) is ≥1°C / min, more preferably 2-10°C / min; Preferably, the temperature of the reaction system after cooling is ≤220°C.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The polymerization reaction temperature in step (5) is 200-220° C. Preferably, the polymerization reaction time in step (5) is 0 to 72 hours, more preferably 0 to 24 hours; Preferably, the temperature of the reaction system after cooling in step (5) is ≤200°C; Preferably, the pressure of the polymerization reaction in step (5) is normal pressure or negative pressure.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The polymerization reaction temperature in step (6) is 120-200° C. Preferably, the polymerization reaction time in step (5) is 0 to 360 hours, more preferably 12 to 120 hours; Preferably, the temperature of the reaction system after cooling in step (5) is ≤60°C; Preferably, the pressure of the polymerization reaction in step (5) is normal pressure or negative pressure.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that The preparation method specifically comprises the following steps: (1) Polymerization stage I: glutaric acid and diamine are dissolved in water to prepare a polyamide salt solution with a mass concentration of 30-90%, and the polymerization reaction is carried out at 150-190° C. in a closed container under a protective gas atmosphere for 0.5-6 hours; Wherein, the molar ratio of glutaric acid to diamine is (0.990-1.005):1; (2) Polymerization stage II: The reaction system obtained in step (1) is subjected to polymerization reaction at 190-230° C. and 0-2.5 MPa for 0.5-6 h; (3) Polymerization stage III: subjecting the reaction system obtained in step (2) to polymerization at 230-270° C. and 0-2.5 MPa for a polymerization time of ≤1 h; (4) Polymerization stage IV: cooling the reaction system obtained in step (3) to a temperature of the reaction system ≤ 220° C., with a cooling rate ≥ 1° C. / min; (5) Polymerization stage V: at 200-220° C. and normal pressure or negative pressure, the reaction system obtained in step (4) is subjected to polymerization reaction for 0-72 hours, and then the temperature is reduced to a temperature of the reaction system ≤ 200° C.; (6) Polymerization stage VI: The reaction system obtained in step (5) is subjected to polymerization reaction at 120-200° C. and normal pressure or negative pressure for 0-360 hours, and then the temperature is reduced to a temperature of the reaction system of ≤60° C. to obtain polyamide.
10. A polyamide prepared by the preparation method according to any one of claims 1 to 9, It is characterized in that The relative viscosity of the polyamide is ≥2.2; Preferably, the number average molecular weight of the polyamide is ≥21000; Preferably, the polyamide includes any one of polyamide 65, polyamide 55, and a copolymer of polyamide 65 and polyamide 55.