Method and device for continuously preparing semi-aromatic polyamide
Through the design of rotating disc solid phase reactor, the problems of poor stability and high energy consumption in the solid phase polymerization process of semi-aromatic polyamide are solved, and high efficiency of high molecular weight products are achieved, which improves production efficiency and product viscosity and stability .
Patent Information
- Application Number
- CN202310542235.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The existing solid-phase polymerization process of semi-aromatic polyamides has problems such as poor batch stability, long production cycle, high energy consumption and low viscosity, and it is difficult to achieve continuous solid-phase polycondensation.
The rotating disc solid phase reactor is used to carry out continuous solid phase tackification reaction, and the design of multiple sets of cutting discs and scrapers achieves uniform spread and push of materials, combined with the inert gas circulation system and heating system, adjust the cutting speed, Temperature and gas flow rate to prepare high molecular weight semiaromatic polyamides.
The process flow is simplified, energy consumption is reduced, production efficiency is improved, semi-aromatic polyamide with suitable viscosity and low yellowness is obtained, the reaction cycle is shortened, and the product stability and processability is improved.
Smart Images

Figure CN118955894A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyamide preparation, and in particular relates to a method and a device for continuously preparing semi-aromatic polyamide. Background Art
[0002] Semi-aromatic polyamide is a special type of polyamide mainly formed by the condensation reaction of aliphatic diamines or dibasic acids with aromatic diamines or dibasic acids. Most of them have a melting point above 300°C. The main varieties include PA6T (polyhexamethylene terephthalamide), PA9T (polynonane terephthalamide), PA10T (polydecane terephthalamide), etc.
[0003] In recent years, semi-aromatic polyamide resins have been widely used in the automotive industry, electronic and electrical industry, aerospace and other fields due to their excellent physical and mechanical properties and processability. At present, semi-aromatic polyamides are restricted by factors such as process or production cost and cannot meet the growing market demand. Semi-aromatic polyamide resins are mainly obtained by prepolymerization of diamines and dibasic acids plus solid phase polymerization process, but the existing solid phase polymerization process has the following problems: Most semi-aromatic polyamide solid phase polymerization processes rely on drum equipment, the process flow is relatively cumbersome, the batch stability is poor, the production process is energy-intensive, and the production efficiency is low; the solid phase polycondensation process mostly adopts an intermittent process, the production cycle is long, the batch stability is poor, and the product viscosity obtained under conventional industrial conditions is low, generally not exceeding 0.85dL / g; it is difficult to achieve continuous solid phase polycondensation of prepolymers.
[0004] CN113227202A discloses a continuous solid-state polymerization process for preparing polyamides derived from diamines and dicarboxylic acids, the method comprising the following steps: feeding a solid diamine dicarboxylate salt into a reaction tower, the reaction tower comprising a continuous multifunctional zone containing a heating section and a degassing section; conveying the salt, or, where applicable, a polymer mixture or polyamide produced by the salt, as a moving packed bed through the continuous multifunctional zone, while, in the heating section, heating the salt, the polymer mixture and the polyamide, respectively, thereby polycondensing the salt to form a polymer mixture, further polycondensing the polymer mixture to form polyamide, and optionally further polycondensing the polyamide to form a polyamide having a higher molecular weight, and generating water vapor, and removing the water vapor through the degassing section; and discharging the obtained polyamide from the reaction tower; wherein the salt, the polymer mixture and the polyamide remain in a solid state. CN113227202A also discloses a reaction tower for a continuous solid-state polycondensation method, wherein the reaction tower comprises at least three continuous multifunctional regions, each of which comprises a heating section and an exhaust section, wherein the heating section comprises a static heat exchanger, and the exhaust section comprises an exhaust device. The document uses a reaction tower for solid-phase polycondensation reaction, and the material is heated unevenly during the polymerization process, and the material near the heating zone is prone to wall adhesion, which not only easily leads to unstable quality between different batches, but also low polymerization efficiency and long polymerization cycle.
[0005] Therefore, there is an urgent need in the art for a method and apparatus for efficiently preparing semi-aromatic polyamide in a solid phase continuously. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention proposes a method and device for continuously preparing semi-aromatic polyamide. In the present invention, the solid phase polycondensation process is relatively simple, the energy consumption is low, and the production efficiency is effectively improved. The operation is simple, and semi-aromatic polyamide with suitable viscosity and low yellowness value can be obtained.
[0007] Specifically, one aspect of the present invention provides a method for preparing a semi-aromatic polyamide, the method comprising the following steps:
[0008] (I) providing semi-aromatic polyamide prepolymer particles;
[0009] (II) Solid-phase polymerization: a rotating disk solid-phase reactor is used to carry out a continuous solid-phase viscosity-increasing reaction on the semi-aromatic polyamide prepolymer particles. The rotating disk solid-phase reactor comprises a rotating disk solid-phase reactor body, a rotating shaft disposed in the rotating disk solid-phase reactor body, a scraper rotating with the rotating shaft, a plurality of groups of feed trays arranged in a vertical direction, a feeding device, a heating system and an inert gas circulation system. The feed trays are disposed in the rotating disk solid-phase reactor body and are used to carry materials. Each group of feed trays comprises an inner tray and an outer tray adjacent to each other in upper and lower directions. The feed tray has a feed hole, the feed hole of the inner tray is arranged near the center of the inner tray, the feed hole of the outer tray is arranged on the periphery of the outer tray, the feeding device is arranged on the top of the rotating disk solid phase reactor body, and is used to feed the semi-aromatic polyamide prepolymer particles to the uppermost feed tray, the scraper is used to push the material on the feed tray, the heating system is used to heat the material on the feed tray, and the inert gas circulation system is used to replace the gas inside the rotating disk solid phase reactor to prepare the semi-aromatic polyamide particles.
[0010] In one or more embodiments, the rotating shaft passes through the center of each discharge tray, and the rotating disk solid phase reactor also has a scraper mounting seat, which is fixed on the rotating shaft. The scraper mounting seat corresponds to the discharge tray one by one, and the scraper mounting seat has one or more evenly distributed spokes. The scraper is fixed on the spokes of the scraper mounting seat, and the scraper is close to the surface of the discharge tray so that the scraper can push the material on the discharge tray when it rotates; preferably, the direction of the scraper is set according to the position of the discharge hole of the discharge tray to ensure that the material moves toward the discharge hole when the scraper rotates.
[0011] In one or more embodiments, the number of groups of the feed trays is 2 to 8, preferably 3 to 8.
[0012] In one or more embodiments, the rotating disk solid phase reactor has a thermal insulation jacket disposed around the rotating disk solid phase reactor body.
[0013] In one or more embodiments, the rotating disk solid phase reactor has a motor and a control system, the rotating shaft is connected to the motor, and the control system controls the rotation speed of the rotating shaft through the motor, thereby adjusting the rotation speed of the scraper.
[0014] In one or more embodiments, the rotating disk solid phase reactor has a dust removal system for removing fine dust in the rotating disk solid phase reactor.
[0015] In one or more embodiments, the rotating disk solid phase reactor has a gas-liquid separator for separating inert gas and moisture.
[0016] In one or more embodiments, the heating system is an inert gas heating system or an electric heating system.
[0017] In one or more embodiments, step (II) includes setting a material feed rate, a heating temperature, a scraper rotation speed, and / or a gas flow rate.
[0018] In one or more embodiments, the particle size of the semi-aromatic polyamide prepolymer particles is no greater than 4 mm.
[0019] In one or more embodiments, the material discharge rate in the rotating disk solid phase reactor is 1 to 3 kg / h.
[0020] In one or more embodiments, the internal temperature of the rotating disk solid phase reactor is no more than 280°C.
[0021] In one or more embodiments, the scraper rotation speed in the rotating disk solid phase reactor is 50 to 200 rpm.
[0022] In one or more embodiments, the gas flow rate in the rotating disk solid phase reactor is controlled to be no more than 3 m / s.
[0023] In one or more embodiments, step (I) comprises the following steps:
[0024] (A) providing a semi-aromatic polyamide salt solution; preferably, a diamine and a dibasic acid are subjected to a salt-forming reaction in the presence of water, a catalyst and a capping agent to obtain a semi-aromatic polyamide salt solution; preferably, the salt-forming reaction temperature is not more than 200° C., and the concentration of the semi-aromatic polyamide salt solution is not more than 85 wt %;
[0025] (B) prepolymerizing the semi-aromatic polyamide salt solution to obtain semi-aromatic polyamide prepolymer particles; preferably, the prepolymerization comprises: stirring the semi-aromatic polyamide salt solution, heating it to 200° C. to 260° C. within 1 to 2 hours during stirring, and continuing to react at a constant pressure of 2.1 to 3.5 MPa for 1 to 1.5 hours.
[0026] Another aspect of the present invention provides a rotating disc solid phase reactor, which includes a rotating disc solid phase reactor body, a rotating shaft arranged in the rotating disc solid phase reactor body, a scraper rotating with the rotating shaft, a plurality of groups of feed trays arranged in a vertical direction, a feeding device, a heating system and an inert gas circulation system, wherein the feed tray is arranged in the rotating disc solid phase reactor body and is used to carry materials, each group of feed trays includes an inner tray and an outer tray adjacent to each other up and down, the feed tray has a feed hole, the feed hole of the inner tray is arranged near the center of the inner tray, and the feed hole of the outer tray is arranged on the periphery of the outer tray, the scraper is used to push the material on the feed tray, the feeding device is arranged at the top of the rotating disc solid phase reactor body and is used to feed semi-aromatic polyamide prepolymer particles to the uppermost feed tray, the heating system is used to heat the material on the feed tray, and the inert gas circulation system is used to replace the gas inside the rotating disc solid phase reactor.
[0027] In one or more embodiments, the rotating disk solid phase reactor is used to implement the method for preparing semi-aromatic polyamide described in any embodiment herein.
[0028] In one or more embodiments, the rotating shaft passes through the center of each discharge tray, and the rotating disk solid phase reactor also has a scraper mounting seat, which is fixed on the rotating shaft. The scraper mounting seat corresponds to the discharge tray one by one, and the scraper mounting seat has one or more evenly distributed spokes. The scraper is fixed on the spokes of the scraper mounting seat, and the scraper is close to the surface of the discharge tray so that the scraper can push the material on the discharge tray when it rotates; preferably, the direction of the scraper is set according to the position of the discharge hole of the discharge tray to ensure that the material moves toward the discharge hole when the scraper rotates.
[0029] In one or more embodiments, the number of groups of the feed trays is 2 to 8, preferably 3 to 8.
[0030] In one or more embodiments, the rotating disk solid phase reactor has a thermal insulation jacket disposed around the rotating disk solid phase reactor body.
[0031] In one or more embodiments, the rotating disk solid phase reactor has a motor and a control system, the rotating shaft is connected to the motor, and the control system controls the rotation speed of the rotating shaft through the motor, thereby adjusting the rotation speed of the scraper.
[0032] In one or more embodiments, the rotating disk solid phase reactor has a dust removal system for removing fine dust in the rotating disk solid phase reactor.
[0033] In one or more embodiments, the rotating disk solid phase reactor has a gas-liquid separator for separating inert gas and moisture.
[0034] In one or more embodiments, the heating system is an inert gas heating system or an electric heating system. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the structure of a rotating disk solid phase reactor in some embodiments of the present invention. Figure 1 In the figure, 1 is the rotating disk solid phase reactor body, 2 is the rotating shaft, 3 is the feeding disk, 4 is the feeding device, 5 is the dust removal system, and 6 is the gas-liquid separator.
[0036] Figure 2 The figures are external views at different angles of the rotating disk solid phase reactor in some embodiments of the present invention.
[0037] Figure 3 Schematic diagrams of the internal feed tray structure at different angles of the rotating disk solid phase reactor in some embodiments of the present invention.
[0038] Figure 4 Schematic diagram of the structure of the inner disk of the rotating disk solid phase reactor in some embodiments of the present invention. Figure 4 In the figure, 7 is a scraper mounting seat, 8 is a spoke, 9 is a scraper, and 10 is a feed hole.
[0039] Figure 5 Schematic diagram of the structure of the outer disk of the rotating disk solid phase reactor in some embodiments of the present invention. Figure 5 In the figure, 7 is a scraper mounting seat, 8 is a spoke, 9 is a scraper, and 10 is a feed hole.
[0040] Figure 6 These are appearance views at different angles of the scraper mounting base in some embodiments of the present invention.
[0041] Figure 7 It is a schematic diagram of the structure of the scraper mounting base and the scraper in some embodiments of the present invention. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0043] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0044] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0045] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0046] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0047] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0048] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0049] The method for preparing semi-aromatic polyamide of the present invention comprises the following steps:
[0050] (I) providing semi-aromatic polyamide prepolymer particles;
[0051] (II) Solid-phase polymerization: A rotating disk solid-phase reactor is used to carry out a continuous solid-phase viscosity-increasing reaction on the semi-aromatic polyamide prepolymer particles to prepare the semi-aromatic polyamide particles.
[0052] The present invention provides a device for preparing semi-aromatic polyamide by solid phase polymerization, namely a rotating disk solid phase reactor. In some embodiments, Figure 1 As shown, the rotating disk solid phase reactor of the present invention comprises:
[0053] Rotating disk type solid phase reactor body 1;
[0054] A rotating shaft 2 is arranged in the rotating disk solid phase reactor body 1;
[0055] Multiple groups of feed trays 3 arranged in the vertical direction are arranged in the rotating disk solid phase reactor body 1 and are used to carry materials. The feed trays 3 have feed holes. Each group of feed trays 3 includes an inner tray and an outer tray adjacent to each other. The feed hole of the inner tray is arranged near the center of the inner tray, and the feed hole of the outer tray is arranged on the periphery of the outer tray.
[0056] A feeding device 4 is arranged on the top of the rotating disk solid phase reactor body 1 and is used to feed the semi-aromatic polyamide prepolymer particles to the uppermost feeding disk 3;
[0057] The scraper rotating with the rotating shaft 2 is used to push the material on the unloading tray 3;
[0058] A heating system, used to heat the material on the lower material tray 3; and
[0059] The inert gas circulation system is used to replace the gas inside the rotating disk solid phase reactor.
[0060] The present invention continuously feeds semi-aromatic polyamide prepolymer particles into the uppermost feeding tray of a rotating disk solid phase reactor through a feeding device, and then the prepolymer is spread on the surface of the feeding tray by a scraper, and is pushed to the feeding hole, and falls onto the next feeding tray, and the cycle is repeated. The temperature of each feeding tray can be set according to the actual process, and the air volume of the inert gas circulation system can be adjusted according to the actual process, and finally a high molecular weight semi-aromatic polyamide is obtained.
[0061] Figure 2 and Figure 3 They are respectively the appearance diagrams of the rotating disk solid phase reactor at different angles and the schematic diagrams of the internal feeding tray structure in some embodiments of the present invention.
[0062] In the present invention, the rotating disk solid phase reactor body is preferably equipped with a heat-insulating jacket.
[0063] In the present invention, the heating system may include an inert gas heating system for heating the inside of the rotating disk solid phase reactor body with an inert gas, and a temperature gradient may be naturally formed inside the rotating disk solid phase reactor body. The heating system may also include an electric heating system, which may control the surface temperature of each feed tray according to demand, such as the top feed tray having a low temperature and the lower layer having a higher temperature. In some embodiments, each feed tray is equipped with an independent heating system, such as an electric heating system, to achieve accurate control of the temperature of each feed tray. The electric heating system may be a heating disc belt arranged inside or at the bottom of the feed tray.
[0064] In the present invention, the rotating shaft is usually arranged to be perpendicular to the horizontal plane. Each unloading tray can be arranged to be parallel to the horizontal plane, or to be arranged to be at a certain angle (for example, ≤30°) to the horizontal plane. The rotating shaft passes through each unloading tray. In some embodiments, the rotating shaft passes through the center of each unloading tray. The scraper is arranged in the rotating disk solid phase reactor body, and each unloading tray is provided with a corresponding scraper. The shape of the scraper needs to ensure that the bottom and the unloading tray are close, for example, it can be a rectangle. The number of scrapers corresponding to each unloading tray is preferably at least 3, for example, 3, 6, 9, 12, 15, and 18. In some embodiments, the rotating disk solid phase reactor has a rotating shaft, a scraper mounting seat and a scraper, the scraper mounting seat is fixed on the rotating shaft, the scraper is fixed on the scraper mounting seat, and the scraper mounting seat corresponds to the unloading tray one by one.
[0065] In some preferred embodiments, the feed tray is divided into an inner tray and an outer tray, and the inner tray and the outer tray are alternately arranged up and down in the rotating disk solid phase reactor body, and an adjacent inner tray and an outer tray form a group of feed trays. In some embodiments, the uppermost feed tray in the rotating disk solid phase reactor is the inner tray. The rotating disk solid phase reactor preferably includes multiple groups of feed trays. Herein, multiple (groups) refers to two (groups) or more than two (groups). The number of groups of feed trays is generally 2 to 8 groups, preferably 3 to 8 groups. The feed tray has a feed hole. The difference between the inner tray and the outer tray is that the positions of the feed holes are different. For example Figure 4 As shown, the inner plate feed hole 10 is arranged near the center of the inner plate, and preferably the distance between the inner plate feed hole 10 and the center of the inner plate does not exceed half of the radius of the inner plate. Figure 5 As shown, the outer plate feed hole 10 is on the periphery of the outer plate, and preferably the distance between the outer plate feed hole 10 and the edge of the outer plate does not exceed half of the radius of the outer plate. The inner plate can be concave with a sunken center, and the outer plate can be convex with a raised center, which is conducive to the movement of materials to the corresponding feed holes. The combined use of the inner and outer plates can promote uniform dispersion of materials, and the purpose of controlling the viscosity of the product can be achieved by controlling the residence time of the materials on the plate surface. Appropriate adjustment of the distance between the inner and outer plates and the distance between the feed plate groups can affect the production efficiency and product viscosity.
[0066] In the present invention, each feeding tray preferably has a plurality of feeding holes. Figure 4 and Figure 5 As shown, each feeding hole is preferably arranged in one or more circles (for example, two circles) along the circumference of the feeding tray, and the feeding holes on each circle are preferably arranged at equal intervals, which is conducive to the material falling evenly into the next layer of the feeding tray. The shape of the feeding hole is preferably circular. The hole diameter of the feeding hole is preferably not more than 8mm, and at the same time needs to be larger than the particle size of the material. For example, the hole diameter of the feeding hole can be 4-8mm. The number of feeding holes is preferably 10-30.
[0067] In some embodiments, such as Figure 4 and Figure 5 As shown, the scraper mounting seat 7 corresponds to the discharge tray one by one, and the scraper mounting seat 7 has one or more (for example, 3 to 6) spokes 8, and the scraper 9 is fixed on the spokes 8 of the scraper mounting seat 7. Preferably, the scraper is close to the disk surface of the discharge tray so that the scraper can spread and push the material on the discharge tray when it rotates. Preferably, the orientation of the scraper is set according to the position of the discharge hole of the discharge tray. For example, the scraper can be at an angle of 15° to 75° with the spokes to ensure that the material moves toward the discharge hole when the scraper rotates. In some embodiments, the direction of the scraper can be adjusted according to the position of the discharge hole. In some embodiments, the center of the scraper mounting seat has a cylindrical structure, which is sleeved on the rotating shaft through the cylindrical structure.
[0068] Figure 6 These are appearance diagrams of the scraper mounting seat at different angles in some embodiments of the present invention, wherein the center of the scraper mounting seat has a cylindrical structure that can be sleeved on a rotating shaft, and the scraper mounting seat has a plurality of (e.g., 3) spokes symmetrically connected to the center of the scraper mounting seat.
[0069] Figure 7 This is a schematic structural diagram of a scraper mounting seat and a scraper in some embodiments of the present invention, wherein the scraper mounting seat has a cylindrical structure at the center, which can be sleeved on a rotating shaft, and the scraper mounting seat has a plurality of (for example, 3) spokes symmetrically connected to the center of the scraper mounting seat, and a plurality of (for example, 4) scrapers are fixed to each spoke.
[0070] In the present invention, the scraper can be connected to the rotating shaft or the scraper mounting seat by bolt connection, pin connection, riveting, welding, adhesive connection and the like.
[0071] In some embodiments, the rotating disk solid phase reactor further includes a cleaning device, which is disposed inside the rotating disk solid phase reactor body and rotates along with the rotating shaft, and is used to clean the material on the unloading disk.
[0072] In the present invention, the rotating disk solid phase reactor may include a motor and a control system. The rotating shaft is connected to the motor. The control system controls the rotating speed of the rotating shaft through the motor, thereby adjusting the rotating speed of the scraper.
[0073] In some embodiments, such as Figure 1 As shown, the inert gas circulation system includes a dust removal system 5 and a gas-liquid separator 6. In some embodiments, the gas-liquid separator 6 has a condensation drain port. Figure 1 The horizontal line at the bottom of the gas-liquid separator 6 represents the condensation drain outlet.
[0074] In the present invention, the inert gas used in the solid phase polymerization process may be N2, CO2, etc.
[0075] The rotating disk solid phase reactor may include a dust removal system for removing suspended matter and fine dust in the rotating disk solid phase reactor. Figure 1 As shown, the dust removal system 5 is connected to the top of the rotating disk solid phase reactor body 1.
[0076] The rotating disk solid phase reactor may also include a gas-liquid separator for separating inert gas and moisture. Figure 1 As shown, the air inlet of the gas-liquid separator 6 is connected to the dust removal system 5 , and the air outlet of the gas-liquid separator 6 is connected to the bottom of the rotating disk solid phase reactor body 1 .
[0077] In a preferred embodiment, the rotating disk solid phase reactor of the present invention is alternately provided with inner and outer disks, and continuous feeding and discharging are achieved by alternately feeding the inner and outer disks to ensure process continuity. The material feeding speed is preferably controlled to be 1 to 3 kg / h, such as 1.5 kg / h, 2 kg / h, 2.5 kg / h, the internal temperature of the rotating disk solid phase reactor is preferably controlled to be no more than 280°C, such as 200 to 280°C, 240 to 280°C, the scraper speed range is preferably 50 to 200 rpm, such as 100 rpm, 150 rpm, and the circulating gas flow (i.e., circulating wind speed) is preferably controlled to be no more than 3 m / s, such as 1 to 3 m / s, 2 to 3 m / s, which is conducive to obtaining semi-aromatic polyamide with suitable viscosity. The solid phase polymerization method of the present invention can shorten the solid phase reaction time to less than 5 hours, such as 1 to 5 hours, 1 to 2.5 hours.
[0078] In the present invention, suitable viscosity means that the intrinsic viscosity of the semi-aromatic polyamide is 0.88 to 0.92 dL / g. When the viscosity is low, the semi-aromatic polyamide has good fluidity, but too low viscosity will make the product strength worse; when the viscosity exceeds 0.92, the semi-aromatic polyamide has poor fluidity, resulting in processing difficulties and limited application.
[0079] In some embodiments, semi-aromatic polyamide prepolymer particles are continuously fed into the first layer (uppermost layer) of the feeding disk of the rotating disk solid phase reactor through a feeding device, and then the prepolymer is evenly spread on the surface of the feeding disk by a scraper and brought to the feeding port and falls onto the next layer of the feeding disk. The feeding is carried out in this way. The temperature of each layer of the feeding disk can be set according to the actual process, and the air volume can be adjusted according to the actual process, so as to finally obtain a semi-aromatic polyamide with suitable viscosity.
[0080] In the present invention, in order to facilitate solid phase polymerization, the particle size of the semi-aromatic polyamide prepolymer particles is preferably no larger than 4 mm. Prepolymer particles with a particle size of no larger than 4 mm can be obtained by controlling the prepolymerization conditions or by crushing.
[0081] In the present invention, the semi-aromatic polyamide prepolymer particles can be prepared by the following method:
[0082] (A) providing a semi-aromatic polyamide salt solution; preferably, a diamine and a dibasic acid are subjected to a salt-forming reaction in the presence of water, a catalyst and a capping agent to obtain a semi-aromatic polyamide salt solution; preferably, the salt-forming reaction temperature is not more than 200° C., for example, it can be 60° C. to 200° C., and the concentration of the semi-aromatic polyamide salt solution is not more than 85 wt %, for example, it can be 40 wt % to 85 wt %, 45 wt %, 50 wt %, 55 wt %, or 60 wt %;
[0083] (B) prepolymerizing the semi-aromatic polyamide salt solution to obtain semi-aromatic polyamide prepolymer particles; preferably, the prepolymerization comprises: stirring the semi-aromatic polyamide salt solution, heating the solution to no more than 260° C., for example, 200° C. to 260° C., 230° C., or 250° C., within 1 to 2 hours, for example, within 1 to 1.5 hours, and continuing the reaction at a constant pressure of 2.1 to 3.5 MPa for 1 to 1.5 hours.
[0084] The dibasic acids applicable to the present invention include aromatic dibasic acids and aliphatic dibasic acids. The aromatic dibasic acids applicable to the present invention include terephthalic acid, isophthalic acid, phthalic acid, etc. The aliphatic dibasic acids applicable to the present invention include adipic acid, azelaic acid, sebacic acid, etc. In the present invention, the dibasic acid used to prepare the semi-aromatic polyamide prepolymer may include an aromatic dibasic acid and an aliphatic dibasic acid in a molar ratio of 80:20 to 20:80.
[0085] Diamines suitable for use in the present invention include compounds having the following molecular formula: H2N-R-NH2, wherein R may be selected from C4-C10 alkylene and C6-C10 arylene. The diamine may include one or more selected from aliphatic diamines and aromatic diamines. Examples of aliphatic diamines include hexamethylenediamine, nonamethylenediamine, decanediamine, and branched isomers of hexamethylenediamine, nonamethylenediamine, and decanediamine. Examples of aromatic diamines include m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, and the like.
[0086] In the present invention, the molar ratio of the dibasic acid to the diamine may be 1:(1 to 1.1).
[0087] The catalyst suitable for the present invention can be a phosphorus-containing catalyst, such as phosphoric acid, phosphorous acid, hypophosphorous acid and metal and non-metal salts thereof. A single catalyst can be used or multiple catalysts can be used in combination. When a phosphorus-containing catalyst is used, the total phosphorus content in the reaction system can be controlled to be 200 to 400 ppm.
[0088] The end-capping agent suitable for the present invention can be a carboxylic acid monofunctional compound such as acetic acid, benzoic acid or a primary amine monofunctional compound such as butylamine. When a carboxylic acid monofunctional compound is used as the end-capping agent, the amount of the end-capping agent can be 0.1-1.5% of the total amount of the dibasic acid.
[0089] In some embodiments, the continuous solid phase method for preparing semi-aromatic polyamide of the present invention comprises the following steps:
[0090] (1) salt formation: a diamine, a dibasic acid, deionized water, a catalyst and a capping agent are placed in a reaction vessel to perform a salt formation reaction to obtain a salt solution. The salt formation reaction temperature is controlled to be no more than 200° C., for example, 60° C. to 200° C., and the concentration of the salt solution is no more than 85 wt %, for example, 40 wt % to 85 wt %;
[0091] (2) Concentration and prepolymerization: Stirring the salt solution, raising the temperature to no more than 260° C., for example, 200° C. to 260° C. within 1 to 2 hours during the stirring process, and continuing the reaction at a constant pressure of 2.1 to 3.5 MPa for 1 to 1.5 hours. After the reaction, the pressure is released to normal pressure to obtain a semi-aromatic polyamide prepolymer, and the particle size of the prepolymer particles does not exceed 4 mm;
[0092] (3) Solid-phase polymerization: A rotating disk solid-phase reactor is used to carry out a continuous solid-phase viscosity-increasing reaction on the semi-aromatic polyamide prepolymer particles. The rotating disk solid-phase reactor has a feeding device, a heating system, a rotating shaft, a scraper rotating with the rotating shaft, and an inert gas circulation system. Semi-aromatic polyamide particles with suitable viscosity are obtained by adjusting the feeding speed, temperature, scraper speed, and inert gas circulation air volume.
[0093] The method and device of the present invention can be used to continuously prepare semi-aromatic polyamides. Typical semi-aromatic polyamides include PA6T, PA6T copolymers (such as PA6T / 66, PA6T / 6, PA6T / 6I, PA6T / 6I / 66, etc.), PA9T, PA10T, etc.
[0094] The present invention has the following beneficial effects:
[0095] (1) The solid phase polycondensation process of the method for continuously preparing semi-aromatic polyamide provided by the present invention is relatively simple, has low energy consumption, effectively improves production efficiency, is simple to operate, and can obtain semi-aromatic polyamide with suitable viscosity, good processability and low yellowness value;
[0096] (2) The present invention provides a solid-phase polymerization device for continuously preparing semi-aromatic polyamides, namely, a rotating disk solid-phase reactor; solid-phase polymerization is carried out by using a feeding disk in cooperation with a rotating scraper, and continuous feeding and discharging is achieved by alternately feeding materials from the inner and outer disks, thereby ensuring process continuity and improving solid-phase polymerization production efficiency; adjacent feeding disks are provided with feeding holes at different positions, and the feeding stability is ensured by adjusting the direction of the scraper; and the parameters of continuous solid-phase polycondensation, including the feeding speed, the internal temperature of the rotating disk solid-phase reactor, the scraper speed, the circulating wind speed, etc., are controlled to achieve efficient preparation of semi-aromatic polyamides with suitable viscosity, good processability, and low yellowness value;
[0097] (3) The present invention continuously feeds semi-aromatic polyamide prepolymer particles into the first layer of the feed tray of the rotating disk solid phase polycondensation reactor through a feeding device, and then the prepolymer is evenly spread on the surface of the feed tray by a scraper and brought to the feed port and falls onto the next layer of the feed tray. In this way, the temperature of each layer of the feed tray can be set according to the actual process, and the air volume can be adjusted according to the actual process. Compared with the existing solid phase equipment, the present invention can obtain high molecular weight semi-aromatic polyamide while shortening the reaction cycle and improving the solid phase polymerization efficiency, and can also obtain products with stable quality.
[0098] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0099] In the present invention, the intrinsic viscosity is tested by dissolving the polymer in a phenol-tetrachloroethane mixed solvent (mass ratio is 3:2) in a 25° C. constant temperature water box according to standard GB / T 12006.2.
[0100] In the present invention, the melting point Tm is tested according to standard ISO11357, and the differential scanning calorimeter (DSC) heating program is: heating to 350°C at a rate of 10°C / min, staying for 5 minutes, then cooling to 25°C at a rate of 10°C / min, staying for 5 minutes, and then heating to 350°C at a rate of 10°C / min. The temperature corresponding to the endothermic peak of the second heating curve is the melting point Tm.
[0101] In the present invention, the content of terminal amine groups and terminal carboxyl groups is quantitatively analyzed and measured by potentiometric titration, and the specific steps are: using a full-automatic point titrator to titrate the content of terminal amine groups or terminal carboxyl groups, taking 1g of polymer and dissolving it in a hexafluoroisopropanol solution, and after the sample is completely dissolved, using a calibrated hydrochloric acid standard solution or KOH-ethanol solution to titrate and test the content of terminal amine groups or terminal carboxyl groups.
[0102] In the present invention, the glass transition temperature Tg is tested according to ISO 11357-2, and the temperature program of the differential scanning calorimeter (DSC) is as follows: the temperature is raised to 350°C at a rate of 20K / min, and the temperature is kept for 5 minutes, the temperature is suddenly cooled to about 50°C lower than the expected glass transition temperature and kept for another 5 minutes, and the temperature is raised again at a heating rate of 20K / min and recorded, and the end point of the temperature program is set to about 30°C higher than the extrapolated melting end temperature (Tefm). The temperature corresponding to the maximum value of the differential DSC signal or the maximum slope of the transition region is Tg.
[0103] In the present invention, the yellowness index (YI) of the sample is tested according to ASTM E313.
[0104] In the present invention, the tensile strength of the sample is tested according to ISO527-2.
[0105] Equipment Examples
[0106] Figure 1 It is a schematic diagram of the structure of the rotating disk solid phase reactor in this equipment example. Figure 4 and Figure 5 They are schematic diagrams of the structures of the inner and outer disks of the rotating disk solid phase reactor in this equipment example. Figure 7It is a structural schematic diagram of the scraper mounting seat and spokes of the rotating disc solid phase reactor in this equipment example. The rotating disc solid phase reactor of this equipment example includes a rotating disc solid phase reactor body 1 with a heat preservation jacket, a rotating shaft 2 arranged in the rotating disc solid phase reactor body 1, a scraper 9 rotating with the rotating shaft 2, six upper and lower material trays 3 with material discharge holes, a feeding device 4, a heating system (not shown), an inert gas circulation system, a scraper mounting seat 7 and spokes 8. The material tray 3 is arranged in the rotating disc solid phase reactor body 1 for carrying materials. The material tray 3 includes 3 groups of inner and outer trays that are alternately arranged up and down and paired in pairs. The uppermost material tray 3 is the inner tray. The material tray 3 is arranged to be parallel to the horizontal plane. The rotating shaft 2 is arranged to be perpendicular to the horizontal plane. The rotating shaft 2 passes through the center of each material tray 3. The scraper mounting seat 7 is fixed on the rotating shaft 2. The scraper mounting seat 7 corresponds to the material tray 3 one by one. The center of the scraper mounting seat 7 has a cylindrical structure, through which the rotating shaft 2 is sleeved. The scraper mounting seat 7 has three spokes 8 that are symmetrically distributed and connected to the cylindrical center. Four scrapers 9 are fixed on each spoke 8. The scrapers 9 are fixed on the spokes 8 of the scraper mounting seat 7. The scrapers 9 are rectangular in shape. Twelve scrapers 9 are correspondingly arranged for each unloading tray 3. The scrapers 9 are close to the disk surface of the unloading tray 3 and are used to spread and push the materials on the unloading tray 3. The unloading holes 10 of the inner tray are arranged near the center of the inner tray, and the unloading holes 10 of the outer tray are arranged on the periphery of the outer tray. Each unloading tray has a plurality of unloading holes 10. The unloading holes 10 are arranged in two circles along the circumference of the unloading tray, and the unloading holes 10 on each circle are arranged at equal intervals. The shape of the unloading hole 10 is circular. The direction of the scraper 9 is set according to the position of the discharge hole 10 of the discharge tray to ensure that the material moves in the direction of the discharge hole 10 when the scraper 9 rotates. The feeding device 4 is arranged at the top of the rotating disk solid phase reactor body 1, and is used to feed the semi-aromatic polyamide prepolymer particles to the uppermost discharge tray 3. The rotating disk solid phase reactor has a motor and a control system (not shown), the rotating shaft 2 is connected to the motor, and the control system controls the speed of the rotating shaft 2 through the motor, thereby adjusting the speed of the scraper 9. The heating system is used to heat the material on the discharge tray 3. The heating system is an inert gas heating system. The inert gas circulation system is used to replace the gas inside the rotating disk solid phase reactor. The inert gas circulation system includes a dust removal system 5 and a gas-liquid separator 6. The inert gas used in the solid phase polymerization process is N2. The air inlet of the dust removal system 5 is connected to the top of the rotating disk solid phase reactor body 1. The dust removal system 5 is used to remove suspended matter and dust in the rotating disk solid phase reactor. The gas-liquid separator 6 is used to separate inert gas and water. The air inlet of the gas-liquid separator 6 is communicated with the air outlet of the dust removal system 5. The air outlet of the gas-liquid separator 6 is communicated with the bottom of the rotating disk solid phase reactor body 1.
[0107] Examples 1-4 used the rotating disk solid phase reactor of this equipment example to carry out the second stage polymerization, the only difference being the number of inner and outer disk groups contained in the rotating disk solid phase reactor.
[0108] Example 1
[0109] Salt formation: 508.3 g (3.06 mol) of terephthalic acid, 365.4 g (2.50 mol) of adipic acid, 658.9 g (5.67 mol) of hexamethylenediamine, 1726.99 g of deionized water, 0.1 g of glacial acetic acid as a capping agent, and 1.04 g of sodium hypophosphite as a catalyst were added to a 5 L high-pressure reactor. After five nitrogen replacements, the reactor was closed, stirring was started, and the temperature in the reactor was controlled at 60°C. The salt formation time was 40 min.
[0110] Concentration and prepolymerization: During the stirring process, the temperature is raised to 250°C within 1.5 hours, and the reaction is continued at a constant pressure for 1 hour, and the pressure is controlled at 3.5 MPa; after the reaction is completed, the pressure is released to normal pressure to obtain a semi-aromatic polyamide prepolymer; the semi-aromatic polyamide prepolymer particles are crushed to a particle size of less than 4 mm;
[0111] Post-stage polymerization: A rotating disk solid-phase reactor with 4 sets of inner and outer disks was used for continuous solid-phase viscosity-increasing reaction. Semi-aromatic polyamide particles were obtained by adjusting the feeding speed, temperature, shaft speed and inert gas circulation volume. The feeding speed of semi-aromatic polyamide prepolymer particles was 3 kg / h, the internal temperature of the rotating disk solid-phase reactor was controlled at 280°C, the rotation speed was 50 rpm, the circulating wind speed was controlled at 3 m / s, and the total solid-phase polymerization time was 2 h.
[0112] The semi-aromatic polyamide finally obtained had a melting point Tm of 305.2° C. and an intrinsic viscosity of 0.89 dL / g.
[0113] Example 2
[0114] Salt formation: 593.1 g (3.57 mol) of terephthalic acid, 322.2 g (1.94 mol) of isophthalic acid, 647.2 g (5.57 mol) of hexamethylenediamine, 1761.9 g of deionized water, 0.2 g of benzoic acid as a capping agent, and 0.5 g of hypophosphorous acid as a catalyst were added to a 5 L high-pressure reactor. After five nitrogen replacements, the reactor was closed, stirring was started, and the temperature in the reactor was controlled at 180°C. The salt formation time was 15 min.
[0115] Concentration and prepolymerization: During the stirring process, the temperature is raised to 230° C. within 1 hour, and the reaction is continued at a constant pressure for 1.2 hours, and the pressure is controlled at 2.7 MPa; after the reaction is completed, the pressure is released to normal pressure to obtain a semi-aromatic polyamide prepolymer; the semi-aromatic polyamide prepolymer particles are crushed to a particle size of less than 4 mm;
[0116] Post-stage polymerization: A rotating disk solid-phase reactor with 8 sets of inner and outer disks was used for continuous solid-phase viscosity-increasing reaction. Semi-aromatic polyamide particles were obtained by adjusting the feeding speed, temperature, shaft speed and inert gas circulation volume. The feeding speed of semi-aromatic polyamide prepolymer particles was 1 kg / h, the internal temperature of the rotating disk solid-phase reactor was controlled at 260°C, the rotation speed was 200 rpm, the circulating wind speed was controlled at 2.8 m / s, and the total solid-phase polymerization time was 2.5 h.
[0117] The semi-aromatic polyamide finally obtained had a melting point Tm of 323° C. and an intrinsic viscosity of 0.91 dL / g.
[0118] Example 3
[0119] Salt formation: 830.6 g (5.0 mol) of terephthalic acid, 815.1 g (5.15 mol) of nonanediamine, 1495.1 g of deionized water, 0.18 g of benzoic acid as a capping agent, and 0.53 g of hypophosphorous acid as a catalyst were added to a 5 L high-pressure reactor. After five nitrogen replacements, the reactor was closed, stirring was started, and the temperature was raised. The temperature in the reactor was controlled at 120°C, and the salt formation time was 30 min.
[0120] Concentration and prepolymerization: During the stirring process, the temperature is raised to 230° C. within 1 hour, and the reaction is continued at a constant pressure for 1.5 hours, and the pressure is controlled at 2.1 MPa; after the reaction is completed, the pressure is released to normal pressure to obtain a semi-aromatic polyamide prepolymer; the semi-aromatic polyamide prepolymer particles are crushed to a particle size of less than 4 mm;
[0121] Post-stage polymerization: A rotating disk solid-phase reactor with three sets of inner and outer disks was used for continuous solid-phase viscosity-increasing reaction. Semi-aromatic polyamide particles were obtained by adjusting the feeding speed, temperature, shaft speed and inert gas circulation volume. The feeding speed of semi-aromatic polyamide prepolymer particles was 2.5 kg / h, the internal temperature of the rotating disk solid-phase reactor was controlled at 240°C, the rotation speed was 150 rpm, the circulating wind speed was controlled at 2.5 m / s, and the total solid-phase polymerization time was 1.8 h.
[0122] The semi-aromatic polyamide finally obtained had a melting point Tm of 304° C. and an intrinsic viscosity of 0.88 dL / g.
[0123] Example 4
[0124] Salt formation: 664.5 g (4.0 mol) of terephthalic acid, 697.9 g (4.05 mol) of decanediamine, 1538.9 g of deionized water, 0.15 g of benzoic acid as a capping agent, and 0.43 g of hypophosphorous acid as a catalyst were added to a 5 L high-pressure reactor. After five nitrogen replacements, the reactor was closed, stirring was started, and the temperature was raised. The temperature in the reactor was controlled at 110° C. The salt formation time was 30 min.
[0125] Concentration and prepolymerization: During the stirring process, the temperature is raised to 230°C within 1 hour, and the reaction is continued at a constant pressure for 1.2 hours, and the pressure is controlled at 2.3 MPa; after the reaction is completed, the pressure is released to normal pressure to obtain a semi-aromatic polyamide prepolymer; the semi-aromatic polyamide prepolymer particles are crushed to a particle size of less than 4 mm;
[0126] Post-stage polymerization: A rotating disk solid-phase reactor with 6 sets of inner and outer disks was used for continuous solid-phase viscosity-increasing reaction. Semi-aromatic polyamide particles were obtained by adjusting the feeding speed, temperature, shaft speed and inert gas circulation volume. The feeding speed of semi-aromatic polyamide prepolymer particles was 1.8 kg / h, the internal temperature of the rotating disk solid-phase reactor was controlled at 240°C, the rotation speed was 120 rpm, the circulating wind speed was controlled at 2 m / s, and the total solid-phase polymerization time was 1 h.
[0127] The semi-aromatic polyamide finally obtained had a melting point Tm of 316° C. and an intrinsic viscosity of 0.89 dL / g.
[0128] Comparative Example 1
[0129] The semi-aromatic polyamide was prepared according to the operation steps described in Example 1, except that the rear polymerization device was replaced with a vacuum drum for solid phase polymerization. When the vacuum drum solid phase process was achieved with the same quality, the time required was 12 hours. The semi-aromatic polyamide finally obtained had a melting point Tm of 305.2°C and an intrinsic viscosity of 0.89 dL / g. The reaction time was much longer than that of Example 1, and the production efficiency was low.
[0130] Comparative Example 2
[0131] The semi-aromatic polyamide was prepared according to the operating steps described in Example 1, except that the feeding rate of the semi-aromatic polyamide prepolymer particles in the later stage polymerization was 0.8 kg / h, and other conditions were kept unchanged. The internal temperature of the rotating disc solid phase reactor was controlled at 280° C., the rotation speed was 50 rpm, the circulating wind speed was controlled at 3 m / s, and the total solid phase polymerization time was 2 h.
[0132] The semi-aromatic polyamide obtained finally has a melting point Tm of 298.3°C and an intrinsic viscosity of 0.94 dL / g. The product is partially cross-linked, the mechanical properties are reduced, the quality is poor, and the product color is seriously yellow, which affects its application.
[0133] Comparative Example 3
[0134] The semi-aromatic polyamide was prepared according to the operating steps described in Example 1, except that the internal temperature of the rotating disc solid phase reactor in the latter stage polymerization was controlled at 290° C., other conditions were kept unchanged, the feeding rate of the semi-aromatic polyamide prepolymer particles was 3 kg / h, the rotation speed was 50 rpm, the circulating wind speed was controlled at 3 m / s, and the total solid phase polymerization time was 2 h.
[0135] The semi-aromatic polyamide obtained finally had a melting point Tm of 306.5°C and an intrinsic viscosity of 1.02 dL / g. The product had a wall-sticking phenomenon, a yellowish color, and a high viscosity, and could not be injection molded.
[0136] Comparative Example 4
[0137] The semi-aromatic polyamide was prepared according to the operating steps described in Example 1, except that the rotation speed in the latter stage polymerization was 220 rpm, keeping other conditions unchanged, the feeding rate of the semi-aromatic polyamide was 3 kg / h, the internal temperature of the rotating disc solid phase reactor was controlled at 280°C, the circulating wind speed was controlled at 3 m / s, and the total solid phase polymerization time was 2 h.
[0138] The semi-aromatic polyamide finally obtained has a melting point Tm of 304.3°C and an intrinsic viscosity of 0.82 dL / g. The mechanical strength of the product is poor.
[0139] The results of preparing semi-aromatic polyamides in Examples 1-4 and Comparative Examples 1-4 are shown in Tables 1 and 2.
[0140] Table 1
[0141]
[0142]
[0143] Table 2
[0144]
Claims
1. A method for preparing semi-aromatic polyamide, characterized in that: The method comprises the following steps: (I) providing semi-aromatic polyamide prepolymer particles; (II) solid phase polymerization: using a rotating disk solid phase reactor to perform a continuous solid phase viscosity increasing reaction on the semi-aromatic polyamide prepolymer particles to prepare semi-aromatic polyamide particles; The rotating disk solid phase reactor comprises a rotating disk solid phase reactor body, a rotating shaft arranged in the rotating disk solid phase reactor body, a scraper rotating with the rotating shaft, a plurality of groups of feed trays arranged in a vertical direction, a feeding device, a heating system and an inert gas circulation system, wherein the feed tray is arranged in the rotating disk solid phase reactor body and is used to carry materials, each group of feed trays comprises an inner tray and an outer tray adjacent to each other up and down, the feed tray has a feed hole, the feed hole of the inner tray is arranged near the center of the inner tray, and the feed hole of the outer tray is arranged at the periphery of the outer tray, the feeding device is arranged at the top of the rotating disk solid phase reactor body and is used to feed semi-aromatic polyamide prepolymer particles to the uppermost feed tray, the scraper is used to push the materials on the feed tray, the heating system is used to heat the materials on the feed tray, and the inert gas circulation system is used to replace the gas inside the rotating disk solid phase reactor.
2. The method according to claim 1, characterized in that The rotating shaft passes through the center of each discharge tray, and the rotating disk solid phase reactor also has a scraper mounting seat, which is fixed on the rotating shaft. The scraper mounting seat corresponds to the discharge tray one by one, and the scraper mounting seat has one or more evenly distributed spokes. The scraper is fixed on the spokes of the scraper mounting seat, and the scraper is close to the disk surface of the discharge tray so that the scraper can push the material on the discharge tray when it rotates; preferably, the direction of the scraper is set according to the position of the discharge hole of the discharge tray to ensure that the material moves toward the discharge hole when the scraper rotates.
3. The method according to claim 1, characterized in that The number of groups of the feeding trays is 2 to 8, preferably 3 to 8.
4. The method according to claim 1, characterized in that The method has one or more of the following features: The rotating disk solid phase reactor has a heat preservation jacket arranged around the rotating disk solid phase reactor body; The rotating disk solid phase reactor has a motor and a control system, the rotating shaft is connected to the motor, and the control system controls the rotation speed of the rotating shaft through the motor, thereby adjusting the rotation speed of the scraper; The rotating disk solid phase reactor has a dust removal system for removing fine dust in the rotating disk solid phase reactor; The rotating disk solid phase reactor has a gas-liquid separator for separating inert gas and water; The heating system is an inert gas heating system or an electric heating system.
5. The method according to claim 1, characterized in that The method has one or more of the following features: The particle size of the semi-aromatic polyamide prepolymer particles does not exceed 4 mm; The material feeding speed in the rotating disk solid phase reactor is 1 to 3 kg / h; The internal temperature of the rotating disk solid phase reactor is no more than 280°C; The scraper speed in the rotating disk solid phase reactor is 50 to 200 rpm; The gas flow rate in the rotating disk solid phase reactor is controlled to be no more than 3 m / s.
6. The method according to claim 1, characterized in that The step (I) comprises the following steps: (A) providing a semi-aromatic polyamide salt solution; preferably, a diamine and a dibasic acid are subjected to a salt-forming reaction in the presence of water, a catalyst and a capping agent to obtain a semi-aromatic polyamide salt solution; preferably, the salt-forming reaction temperature is not more than 200° C., and the concentration of the semi-aromatic polyamide salt solution is not more than 85 wt %; (B) prepolymerizing the semi-aromatic polyamide salt solution to obtain semi-aromatic polyamide prepolymer particles; preferably, the prepolymerization comprises: stirring the semi-aromatic polyamide salt solution, heating it to 200° C. to 260° C. within 1 to 2 hours during stirring, and continuing to react at a constant pressure of 2.1 to 3.5 MPa for 1 to 1.5 hours.
7. A rotating disk solid phase reactor for implementing the method according to claim 1, characterized in that: The rotating disk solid phase reactor comprises a rotating disk solid phase reactor body, a rotating shaft arranged in the rotating disk solid phase reactor body, a scraper rotating with the rotating shaft, a plurality of groups of feed trays arranged in a vertical direction, a feeding device, a heating system and an inert gas circulation system, wherein the feed tray is arranged in the rotating disk solid phase reactor body and is used to carry materials, each group of feed trays comprises an inner tray and an outer tray adjacent to each other up and down, the feed tray has a feed hole, the feed hole of the inner tray is arranged near the center of the inner tray, and the feed hole of the outer tray is arranged at the periphery of the outer tray, the feeding device is arranged at the top of the rotating disk solid phase reactor body and is used to feed semi-aromatic polyamide prepolymer particles to the uppermost feed tray, the scraper is used to push the materials on the feed tray, the heating system is used to heat the materials on the feed tray, and the inert gas circulation system is used to replace the gas inside the rotating disk solid phase reactor.
8. The rotating disk solid phase reactor according to claim 7, characterized in that: The rotating shaft passes through the center of each discharge tray, and the rotating disk solid phase reactor also has a scraper mounting seat, which is fixed on the rotating shaft. The scraper mounting seat corresponds to the discharge tray one by one, and the scraper mounting seat has one or more evenly distributed spokes. The scraper is fixed on the spokes of the scraper mounting seat, and the scraper is close to the disk surface of the discharge tray so that the scraper can push the material on the discharge tray when it rotates; preferably, the direction of the scraper is set according to the position of the discharge hole of the discharge tray to ensure that the material moves toward the discharge hole when the scraper rotates.
9. The rotating disk solid phase reactor according to claim 7, characterized in that: The number of groups of the feeding trays is 2 to 8, preferably 3 to 8.
10. The rotating disk solid phase reactor according to claim 7, characterized in that: The rotating disk solid phase reactor has one or more of the following features: The rotating disk solid phase reactor has a heat preservation jacket arranged around the rotating disk solid phase reactor body; The rotating disk solid phase reactor has a motor and a control system, the rotating shaft is connected to the motor, and the control system controls the rotating speed of the rotating shaft through the motor, thereby adjusting the rotating speed of the scraper; The rotating disk solid phase reactor has a dust removal system for removing fine dust in the rotating disk solid phase reactor; The rotating disk solid phase reactor has a gas-liquid separator for separating inert gas and water; The heating system is an inert gas heating system or an electric heating system.