Preparation method of intumescent organic-inorganic coated flame retardant polyurethane foam
The expanded organic-inorganic coated flame retardant prepared by materials such as polyphosphamide, melamine and β-cyclodextrin combined with the reaction mechanism of high content of phosphorus and nitrogen elements, solves the flammability problem of polyurethane foam and realizes the Highly efficient flame retardant properties and environmentally friendly polyurethane foam material.
Patent Information
- Application Number
- CN202411031328.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The high flammability of polyurethane foam and the toxic flue gas released during combustion pose a threat to the safety of life and property. The existing halogen-free flame retardants have shortcomings in their environmental friendliness and flame retardant properties.
采用聚磷酰胺、三聚氰胺和β-环糊精等材料制备膨胀型有机-无机包覆阻燃剂,通过β-环糊精包覆纳米氢氧化镁,结合高含量磷、氮元素的反应机制,形成保护层以提高阻燃性能,并在一定程度上缓解纳米氢氧化镁对聚氨酯的负面效果。
The flame retardant performance of polyurethane foam is significantly improved, the combustion temperature is reduced, the carbon layer is formed to suppress combustion, and while maintaining physical properties, the use of nanomagnesium hydroxide is reduced, achieving environmentally friendly flame retardant effect.
Smart Images

Figure BDA0004969997610000021 
Figure BDA0004969997610000061 
Figure BDA0004969997610000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyurethane, and in particular to a method for preparing an expanded polyurethane foam coated with an organic-inorganic flame retardant. Background Art
[0002] Polyurethane foam, or PUF for short, is a widely used foam material. Its excellent physical and chemical properties make it irreplaceable in many fields. However, the high flammability of PUF and the large amount of heat and toxic smoke released when it burns pose a serious threat to people's lives and property. Therefore, how to improve the flame retardant properties of PUF and solve its fire risk from the source has become an important topic in scientific research and industry.
[0003] Polyurethane foam is a material made of isocyanate and hydroxyl compounds. It can be divided into two categories according to its hardness: soft (FPUF) and hard (RPUF). PUF has many advantages, but its high flammability is a major hidden danger in its application. PUF contains a large number of flammable hydrocarbon segments and porous structures, resulting in its limiting oxygen index (LOI) of only 17-19%, and releases a large amount of heat and toxic fumes (CO, HCN, NO, etc.) when burning. These toxic fumes are extremely harmful to human health and may cause fire accidents, posing a serious threat to people's lives and property.
[0004] In order to solve the flame retardant problem of PUF, scientific researchers have conducted a lot of research and exploration. Among them, adding flame retardants is a conventional and reliable method to improve the flame retardant properties of PUF. Flame retardants can reduce the burning speed and fire spread speed of foam by absorbing heat, releasing non-combustible gases, and generating flame retardant layers when the foam burns, thereby achieving the purpose of flame retardancy. Adding flame retardants containing halogen elements, even if the flame retardancy is good, will produce harmful gases and pollute the atmospheric environment. At present, the development of halogen-free and harmless flame retardants is the key to flame retardant polyurethane. To develop towards environmentally friendly development, the development of a reactive halogen-free flame retardant is in line with the current development direction. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing an intumescent organic-inorganic coated flame retardant polyurethane foam. The intumescent organic-inorganic coated flame retardant prepared by the present invention is prepared from polyphosphoramide, melamine, β-cyclodextrin and nano magnesium hydroxide, which not only has good flame retardant properties, but also utilizes β-cyclodextrin to coat nano magnesium hydroxide, which can alleviate the negative effects of nano magnesium hydroxide on polyurethane to a certain extent.
[0006] The present invention provides a method for preparing an expandable polyurethane foam coated with an organic-inorganic flame retardant, comprising the following steps:
[0007] Step 1: dissolve β-cyclodextrin in an organic solvent, add ammonium polyphosphate (APP), melamine (MEL), and a surfactant, stir evenly, and obtain a liquid nitrogen-phosphorus flame retardant solution.
[0008] Step 2: Grind nano magnesium hydroxide and add it to water, add it to the above milky white solution after ultrasonic treatment, and continue ultrasonic treatment to obtain a liquid organic-inorganic coated nitrogen-phosphorus intumescent flame retardant.
[0009] Step 3: Mix the liquid organic-inorganic coated nitrogen-phosphorus intumescent flame retardant with the polyurethane foam emulsion and the polyurethane foaming aid, stir, and ultrasonically disperse until a milky white solution is obtained, and foam and mature to obtain an intumescent organic-inorganic coated flame retardant polyurethane foam.
[0010] The present invention uses polyphosphoramide, melamine, and β-cyclodextrin to prepare a nitrogen-phosphorus intumescent flame retardant, wherein ammonium polyphosphate is used as an acid source, melamine is used as a gas source, and β-cyclodextrin is selected as a carbon source. The nitrogen-phosphorus intumescent flame retardant contains high content of phosphorus and nitrogen elements, has better flame retardant properties than traditional multi-carbon flame retardants, has a higher decomposition temperature, generates phosphoric acid, nitrogen, etc., which will take away a large amount of heat energy, thereby reducing the temperature during combustion; it can also promote the carbonization process of combustibles, form a carbon layer, and prevent combustibles from contacting with oxygen, thereby inhibiting combustion. Phosphorus and nitrogen can react with combustibles and form a protective layer together with carbon, effectively improving the thermal stability of combustibles.
[0011] The present invention selects β-cyclodextrin as the carbon source, and the conical hollow cylindrical three-dimensional ring structure presented by cyclodextrin. In the hollow structure, the lower end (smaller open end) is composed of the hydrophilic group C6, and the upper end (larger open end) is composed of C2 and C3 cis hydrogen groups, which have a certain hydrophilicity, and the shielding of the CH bond forms a hydrophobic area in the cavity. This structure results in the cyclodextrin structure having no reducing end and no non-reducing end, which makes it stable in alkaline media and causes cracking in strong acids. Its unique cavity structure allows it to encapsulate small molecules of a certain size, bringing about a certain host-guest synergy.
[0012]
[0013] Nano magnesium hydroxide is a good flame retardant, but it often needs to be added in a very high content to have excellent flame retardant properties. Too much nano magnesium hydroxide content will lead to reduced physical properties of polyurethane, thus affecting its use. The present invention finds that the cyclodextrin structure encapsulates nano magnesium hydroxide in the cavity, which can alleviate the negative effects of nano magnesium hydroxide on polyurethane to a certain extent.
[0014] In addition, the present invention finds that the types and proportions of β-cyclodextrin, ammonium polyphosphate, melamine and inorganic flame retardant filler have an important influence on the flame retardant properties of the product. Finally, the present invention finds through experiments that when the mass ratio of β-cyclodextrin, ammonium polyphosphate, melamine and inorganic flame retardant filler is 10:15-20:5-10:15-20, and the inorganic flame retardant filler is nano magnesium hydroxide, the flame retardant properties of polyurethane foam are the best.
[0015] Preferably, in step 1: the organic solvent is acetone.
[0016] Preferably, in step 1: the dosage ratio of the β-cyclodextrin to the organic solvent is 10 g: 25-50 mL.
[0017] Preferably, in step 1: the mass ratio of the β-cyclodextrin to the surfactant is in the range of 100:5-15.
[0018] Preferably, in step 1: the surfactant is TX-10.
[0019] Preferably, in step 1: the stirring speed is 300-600 rpm, and the time is 1-3 h.
[0020] Preferably, in step 2: the particle size of the nano magnesium hydroxide after grinding is 8-15 nm.
[0021] Preferably, in step 3: the mass ratio of the organic-inorganic coated nitrogen-phosphorus intumescent flame retardant to the polyurethane foam emulsion and the polyurethane foaming aid is in the range of 30:60-80:3-7.
[0022] Preferably, in step 3: the solid content of the polyurethane foam emulsion is 20-30wt%.
[0023] Preferably, in step 3: the polyurethane foaming aid is FOCAT-8003M.
[0024] Compared with the prior art, the beneficial effects of the present invention are:
[0025] (1) The intumescent organic-inorganic coated flame retardant of the present invention is prepared from polyphosphorus amide, melamine, β-cyclodextrin and nano-magnesium hydroxide. Among them, ammonium polyphosphate is used as an acid source, melamine is used as a gas source, and β-cyclodextrin is selected as a carbon source. The flame retardant contains high content of phosphorus and nitrogen elements, has good flame retardant properties, a higher decomposition temperature, and generates phosphoric acid, nitrogen, etc., which will take away a large amount of heat energy, thereby reducing the temperature during combustion; it can also promote the carbonization process of combustibles, form a carbon layer, and prevent combustibles from contacting with oxygen, thereby inhibiting combustion. Phosphorus and nitrogen can react with combustibles and form a protective layer together with carbon, which effectively improves the thermal stability of combustibles.
[0026] (2) The present invention utilizes β-cyclodextrin to coat nano-magnesium hydroxide, which can alleviate the negative effects of nano-magnesium hydroxide on polyurethane to a certain extent. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the embodiments.
[0028] Example 1 (the mass ratio of β-cyclodextrin, ammonium polyphosphate, melamine and nano magnesium hydroxide is 10:18:8:18)
[0029] Step 1: Dissolve 10 g of β-cyclodextrin in 50 ml of acetone, add 18 g of ammonium polyphosphate (APP), 8 g of melamine (MEL), and 1 g of surfactant TX-10, stir evenly to obtain a liquid nitrogen-phosphorus flame retardant solution.
[0030] Step 2: Grind 18 g of nano magnesium hydroxide to 8-15 nm and add it to 20 ml of water. After ultrasonic treatment for 15 min, add it to the above milky white solution and continue ultrasonic treatment for 30 min to obtain a liquid organic-inorganic coated nitrogen-phosphorus intumescent flame retardant.
[0031] Step 3: Mix the liquid organic-inorganic coated nitrogen-phosphorus intumescent flame retardant with a mass ratio of 30:70:5 with the polyurethane foam emulsion (solid content 25wt%) and the polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained, add the foaming aid and mature to obtain an intumescent organic-inorganic coated flame retardant polyurethane foam.
[0032] Comparative Example 1 (without β-cyclodextrin: the mass ratio of ammonium polyphosphate, melamine and nano magnesium hydroxide is 18:8:18)
[0033] Step 1: In 50 ml of acetone, add 18 g of ammonium polyphosphate (APP), 8 g of melamine (MEL), and 1 g of surfactant TX-10, and stir evenly to obtain a liquid nitrogen-phosphorus flame retardant solution.
[0034] Step 2: Grind 18g of nano magnesium hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0035] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0036] Comparative Example 2 (no ammonium polyphosphate: the mass ratio of β-cyclodextrin, melamine and nano magnesium hydroxide is 10:8:18)
[0037] Step 1: In 50 ml of acetone, add 10 g of β-cyclodextrin, 8 g of melamine (MEL), and 1 g of surfactant TX-10, and stir evenly to obtain a liquid nitrogen-phosphorus flame retardant solution.
[0038] Step 2: Grind 18g of nano magnesium hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0039] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0040] Comparative Example 3 (without melamine: the mass ratio of β-cyclodextrin, ammonium polyphosphate and nano magnesium hydroxide is 10:18:18)
[0041] Step 1: In 50 ml of acetone, add 10 g of β-cyclodextrin, 18 g of ammonium polyphosphate (APP), and 1 g of surfactant TX-10, and stir evenly to obtain a nitrogen-phosphorus flame retardant solution.
[0042] Step 2: Grind 18g of nano magnesium hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0043] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0044] Comparative Example 4 (no nano magnesium hydroxide: the mass ratio of β-cyclodextrin, ammonium polyphosphate and melamine is 10:18:8)
[0045] Step 1: Dissolve 10 g of β-cyclodextrin in 50 ml of acetone, add 18 g of ammonium polyphosphate (APP), 8 g of melamine (MEL), and 1 g of surfactant TX-10, stir evenly to obtain a liquid nitrogen-phosphorus flame retardant solution.
[0046] Step 2: Mix a nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained, add a foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam comparative example 5 (too little nano magnesium hydroxide: the mass ratio of β-cyclodextrin, ammonium polyphosphate, melamine and nano magnesium hydroxide is 10:18:8:5);
[0047] Step 1: In 50 ml of acetone, add 10 g of β-cyclodextrin, 18 g of ammonium polyphosphate (APP), and 1 g of surfactant TX-10, and stir evenly to obtain a nitrogen-phosphorus flame retardant solution.
[0048] Step 2: Grind 5g of nano magnesium hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0049] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0050] Comparative Example 6 (too much nano magnesium hydroxide: the mass ratio of β-cyclodextrin, ammonium polyphosphate, melamine and nano magnesium hydroxide is 10:18:8:25);
[0051] Step 1: In 50 ml of acetone, add 10 g of β-cyclodextrin, 18 g of ammonium polyphosphate (APP), and 1 g of surfactant TX-10, and stir evenly to obtain a nitrogen-phosphorus flame retardant solution.
[0052] Step 2: Grind 25g of nano magnesium hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0053] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0054] Comparative Example 7 (using nano aluminum hydroxide: β-cyclodextrin, ammonium polyphosphate, melamine and nano aluminum hydroxide in a mass ratio of 10:18:8:18);
[0055] Step 1: In 50 ml of acetone, add 10 g of β-cyclodextrin, 18 g of ammonium polyphosphate (APP), and 1 g of surfactant TX-10, and stir evenly to obtain a nitrogen-phosphorus flame retardant solution.
[0056] Step 2: Grind 18g of nano aluminum hydroxide to 8-15nm and add it to 20ml of water. After ultrasonic treatment for 15min, add it to the above milky white solution and continue ultrasonic treatment for 30min to obtain a liquid organic-inorganic nitrogen-phosphorus intumescent flame retardant.
[0057] Step 3: Mix an organic-inorganic nitrogen-phosphorus flame retardant solution with a mass ratio of 30:70:5 with a polyurethane foam emulsion (solid content 25wt%) and a polyurethane foaming aid FOCAT-8003M, stir for more than 30 minutes, and ultrasonically disperse for 30 minutes until a milky white solution is obtained. Add the foaming aid and mature to obtain an expandable organic-inorganic coated flame retardant polyurethane foam.
[0058] Performance Testing
[0059]
[0060]
[0061] By comparing the physical properties of Example 1 with those of Comparative Example 1, it can be seen that cyclodextrin-coated magnesium hydroxide can effectively alleviate the negative impact of magnesium hydroxide on polymers. The polyurethane foam without cyclodextrin coating and magnesium hydroxide has significantly reduced foam pores and decreased mechanical properties, while the polyurethane foam with cyclodextrin-coated magnesium hydroxide has larger pores and better mechanical properties. It can be seen that cyclodextrin-coated magnesium hydroxide can alleviate the negative impact on polyurethane foam to a certain extent, and can also retain the excellent flame retardant properties of magnesium hydroxide.
[0062] By comparing Comparative Examples 2-4, we can find out the effects of ammonium polyphosphate, melamine, cyclodextrin and magnesium hydroxide on flame retardancy. The reduction of APP in other comparative examples reduces the flame retardancy, indicating that APP provides the main flame retardancy. The reduction of cyclodextrin reduces the coating effect of polyurethane emulsion on magnesium hydroxide, reducing the physical properties of polyurethane foam. Because of its unique triazine ring structure, melamine does not need a particularly large amount to have excellent flame retardancy. Too much inorganic filler will reduce the mechanical properties of polyurethane and reduce porosity, which is not worth the loss. It is not easy to add too much, and it must be matched with the amount of cyclodextrin to obtain the best flame retardant performance.
[0063] Comparative Example 7 shows that although nano aluminum hydroxide also has good flame retardant properties, magnesium hydroxide has a better flame retardant effect than aluminum hydroxide, because the decomposition heat of magnesium hydroxide is higher than that of aluminum hydroxide and can withstand higher temperatures, and can exhibit better flame retardant properties in polyurethane foam.
[0064] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing an intumescent polyurethane foam coated with an organic-inorganic flame retardant, characterized in that The following steps are involved: Step 1: dissolve β-cyclodextrin in an organic solvent, add ammonium polyphosphate, melamine, and a surfactant, and stir evenly to obtain a milky white solution; Step 2: Grind nano magnesium hydroxide and add it to water, add it to the above milky white solution after ultrasonic treatment, and continue ultrasonic treatment to obtain a liquid organic-inorganic coated nitrogen-phosphorus intumescent flame retardant; The mass ratio of the β-cyclodextrin, ammonium polyphosphate, melamine and nano magnesium hydroxide is 10:15-20:5-10:15-20; Step 3: Mix the organic-inorganic coated nitrogen-phosphorus intumescent flame retardant with the polyurethane foam emulsion and the polyurethane foaming aid, stir, and ultrasonically disperse until a milky white solution is obtained, and foam and mature to obtain an intumescent polyurethane foam of the organic-inorganic coated flame retardant.
2. The preparation method according to claim 1, characterized in that: In step 1: the organic solvent is acetone.
3. The preparation method according to claim 1 or 2, characterized in that: In step 1: the dosage ratio of the β-cyclodextrin to the organic solvent is 10 g: 25-50 mL.
4. The preparation method according to claim 1, characterized in that: In step 1: the mass ratio of the β-cyclodextrin to the surfactant is 100:5-15.
5. The preparation method according to claim 1, characterized in that: In step 1: the surfactant is TX-10.
6. The preparation method according to claim 1, characterized in that: In step 1: the stirring speed is 300-600 rpm, and the time is 1-3 h.
7. The preparation method according to claim 1, characterized in that: In step 2: the particle size of the nano magnesium hydroxide after grinding is 8-15 nm.
8. The preparation method according to claim 1, characterized in that: In step 3: the mass ratio of the organic-inorganic coated nitrogen-phosphorus intumescent flame retardant to the polyurethane foam emulsion and the polyurethane foaming aid is 30:60-80:3-7.
9. The preparation method according to claim 1, characterized in that: In step 3: the solid content of the polyurethane foam emulsion is 20-30wt%.
10. The preparation method according to claim 1, characterized in that: In step 3: the polyurethane foaming aid is FOCAT-8003M.