Preparation method of novel gallium adsorption porous chelating resin for supercritical CO2-assisted amidoximation

By swelling and aminoxilated porous microspheres in supercritical CO2, the problems of low aminoxilation and long process consumption of porous resins are solved, and efficient gallium adsorption and analysis are achieved, improving gallium recovery efficiency and product quality.

CN118955997APending Publication Date: 2024-11-15GUIZHOU HAIHAO NEW MATERIALS CO LTD +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411015949.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art cannot effectively improve the degree of aminoxidation on the surface of porous chelating resin spheres and inside micropores, resulting in low gallium recovery efficiency, long swelling process and excessive solvent use, affecting product quality.

Method used

The supercritical CO2-assisted amidoximetization process is adopted to promote the penetration and diffusion of amidoximetization reagent by swelling porous microspheres in supercritical CO2, improve the efficiency of amidoximetization reaction and shorten the production cycle.

Benefits of technology

The degree of aminoximetization and gallium adsorption of the porous resin are significantly improved, the swelling and aminoximetization time is shortened, the solvent usage is reduced, the adsorption rate and analytical efficiency of the gallium are improved, and the product quality is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955997A_ABST
    Figure CN118955997A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of novel gallium adsorption porous chelating resin for supercritical CO2-assisted ammoximation. The preparation method comprises two parts, namely preparation of porous chelating resin beads and ammoximation of the supercritical CO2-assisted resin beads. The problem that the amidoximation degree on the surface of a porous chelate resin sphere and in micropores cannot be improved in a feasible, operable and quantitative mode in the prior art is solved. Belongs to the field of material preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a novel gallium-adsorbing porous chelating resin assisted by supercritical CO2 amine oximation, and belongs to the field of material preparation. Background Art

[0002] Gallium is an important rare metal. Gallium compounds are high-quality semiconductor materials and are widely used in optoelectronics, microwave communications, aerospace, electronics, new energy materials and devices, and other fields. Except for the extremely rare gallium-sulfide copper ore, metallic gallium can hardly be independently ore-formed. Metallic gallium is always associated with bauxite. Currently, more than 90% of the gallium metal in the world is extracted from the Bayer process circulating mother liquor of bauxite, and almost more than 90% of the gallium recovery industry is in China. Among the currently industrialized process methods, the use of acid-based chelating resin adsorption to recover gallium has the advantages of simple process, low requirements for gallium metal concentration in the circulating mother liquor, high recovery rate, and easy large-scale industrial production, and is the most widely used.

[0003] The chelating resins currently used in China are all prepared by a two-step process. First, monomers, crosslinking agents, initiators, dispersants, and porogens are polymerized in a saline medium to form porous microspheres. Then, based on the porous microspheres, the surface of the porous microspheres is oximated with an oximation agent. The oximated microspheres use oxime groups (-N-OH) and amine groups (-NH2) to complex the gallium metal in the Bayer process circulating mother liquor and recover the gallium.

[0004] At present, the polymerization monomer of the amine oxime chelating resin is acrylonitrile (AN), and the crosslinking agent is generally divinylbenzene (DVB). These two monomers are polymerized into skeleton spheres through suspension polymerization. A small amount of a third monomer is used to enhance the strength of the skeleton spheres during the preparation process. After the polymer skeleton spheres are prepared, the skeleton spheres are subjected to amine oxime with reagents such as hydroxylamine sulfate, hydroxylamine hydrochloride, ammonium sulfate, and ammonium chloride.

[0005] During the amine oximation process, the penetration of the amine oximation reagent into the resin sphere is crucial. The chelating resin prepared by the suspension polymerization of acrylonitrile (AN) and divinylbenzene (DVB) not only has unstable bead resin strength, but also has difficult to control surface pore structure. It is particularly important that the skeleton sphere must be fully swollen with an appropriate solvent before the amine oximation of the sphere to ensure that the amine oximation reagent can fully penetrate and amine oximate the sphere resin. Under the current process conditions, it is extremely difficult for the amine oximation reagent to penetrate into the pores of the resin sphere, and the amine oximation reaction only occurs on the surface of the sphere resin. This results in a low degree of amine oximation of the chelating resin, and the saturated adsorption capacity of the resin decreases by more than 70% after 15 adsorption cycles.

[0006] In the current process, the swelling time of the skeleton sphere is mainly prolonged by the solvent, so that the sphere is fully swollen to ensure that the amine oximation reagent can diffuse into the sphere during the subsequent amine oximation process. This process not only requires the use of a large amount of pre-treatment solvent, but also has a long swelling time, usually more than 3 hours. More importantly, this swelling process not only causes great use and waste of solvent, but also lacks quantitative monitoring, which seriously affects the product quality of the amine oximation chelating resin.

[0007] Porous chelating resins rely on uniform pore structure and co-amine oximation on the surface and inside the pores to improve gallium adsorption. However, there is no feasible, operable, and quantitative process reported so far to improve the degree of amine oximation on the surface and inside the micropores of porous chelating resin spheres. Therefore, seeking a high-strength new microporous chelating resin for efficient and long-term adsorption of gallium metal in the Bayer process circulating mother liquor has become one of the important research directions in the current gallium metal recovery industry. Summary of the invention

[0008] The invention provides a method for preparing a novel gallium-adsorbed porous chelating resin assisted by supercritical CO2 amine oximation, so as to solve the problem that the current process cannot improve the amine oximation degree on the surface of the porous chelating resin sphere and inside the micropores in a feasible, operable and quantitative manner.

[0009] In order to solve the above problems, a method for preparing a novel gallium adsorbing porous chelating resin assisted by supercritical CO2 amine oximation is proposed, which includes two parts: preparation of porous chelating resin beads and supercritical CO2 assisted amine oximation of resin beads.

[0010] The raw materials for preparing the porous chelating resin beads include, by weight, 5-20% of a main monomer, 1-5% of a modified monomer, 1-10% of a cross-linking monomer, 5-25% of a porogen, 0.5-5% of an initiator accounting for the total weight of the main monomer and the cross-linking monomer, 0.5-10% of a dispersant, and 20-80% of salt water;

[0011] The salt water includes one or two of calcium chloride, sodium chloride and sodium nitrite, and the purity thereof is above 99%; the dispersant is one or two of gelatin and polyvinyl alcohol;

[0012] The main monomer is acrylonitrile; the modified monomer is one or more of styrene, acrylic acid, methyl methacrylate, and hydroxyethyl methacrylate; the crosslinking monomer includes one or more of divinylbenzene, butylated acrylamide, N-butoxymethyl acrylamide, and hydroxyethyl acrylamide; the porogen includes one or more of toluene, paraffin, xylene, and aviation kerosene; the initiator is one or more of benzoyl peroxide and azobisisobutyronitrile;

[0013] Step 1: First, add a certain amount of brine into the reactor according to the ratio, then add a certain amount of dispersant, stir until the dispersant is completely dissolved, and then heat the reactor to the set temperature;

[0014] Step 2: Add the main monomer, cross-linking monomer, modified monomer, porogen, and initiator into the reactor according to the ratio, control the stirring speed, increase the stirring speed after the materials are completely dissolved, and carry out suspension polymerization by step-by-step heating. After the reaction is completed, neutralize the solution after the reaction, filter the product, and finally dry the product with a mesh size below 60 in a dryer at low temperature, remove the porogen, wash the microspheres, and dry them to obtain porous microsphere beads;

[0015] Step 3: Add the copolymeric porous microsphere beads obtained in step 2 to a supercritical CO2 reactor, and control the supercritical CO2 reaction temperature, time, and pressure to allow the pore structure of the microsphere to swell fully;

[0016] Step 4: Add the swollen porous microsphere beads and the amine oxime reagent to the reaction medium in proportion, move the whole into the supercritical CO2 reactor after infiltration, control the supercritical CO2 reaction temperature, time and pressure, and after the reaction is completed, cool the reaction system to below 30°C and discharge the material;

[0017] Step 5: Discharge the mixture obtained in step 4, filter out the solution with a filter, then wash the obtained product with water for multiple times, then filter and dry the water, and dry at low temperature to obtain the amine oxime porous microspheres.

[0018] In step 2, the suspension polymerization is carried out by stage heating. Specifically, the temperature is raised to 75±2°C and kept warm for 2-3 hours; then the temperature is raised to 85±2°C and kept warm for 2-3 hours; finally, the temperature is raised to 95±2°C and kept warm for 2-3 hours.

[0019] Step three is supercritical CO2-assisted swelling of porous microspheres. Effective swelling of porous microspheres can facilitate the subsequent infiltration of amine oxime reagents into the spheres and amine oxime reaction. The supercritical CO2-assisted swelling conditions of porous microspheres are 12-15Mpa, 30-45°C, and 30-60min.

[0020] Step four is the supercritical CO2-assisted swellable porous microspheres amine oximation process, the swollen porous microspheres are taken and added to the batching kettle in proportion, the mass fraction of the beads in the batching kettle is 35-55%, the reaction medium is one or two of water and ethanol, and the mass fraction of the reaction medium is 20-40%; the oximation reagent is one or two of hydroxylamine hydrochloride and hydroxylamine sulfate, and its mass fraction is 10-25%. After the whole system is soaked for 1 hour, it is moved into the supercritical CO2 reactor as a whole. The reaction conditions are 12Mpa-15Mpa, 50-60℃, 3-4 hours, and the amine oximation of the microspheres is completed.

[0021] In step 5, the obtained product is washed with water for multiple times until the pH value is 7, and the cleaning agent used is an aqueous solution of a mixture of sodium hydroxide and sodium carbonate with a mass fraction of 8%.

[0022] In the above preparation method, in step 1, the main monomer and the cross-linking monomer must be deblocked with 5-10% sodium hydroxide solution before use.

[0023] Compared with the prior art, the present invention uses supercritical CO2 to assist the swelling of porous microspheres. This process can not only effectively utilize the penetration and swelling effect of supercritical CO2 to effectively swell the pore structure of the porous microspheres, but the swollen porous resin can also effectively adsorb the amine oximation reagent and carry out amine oximation reaction; more importantly, compared with the traditional solvent immersion swelling process for porous resin, the use of supercritical CO2 swelling process can reduce the swelling time from more than 3 hours to less than 1 hour, greatly shortening the operation time.

[0024] The process of oximation of porous microspheres assisted by supercritical CO2 will not only not cause any damage to the porous structure of the microspheres, but also more effectively promote the penetration and diffusion of oximation reagents into the micropores. This process of oximation of porous microspheres assisted by supercritical CO2 can not only greatly improve the oximation reaction on the surface of the resin microspheres, but also can infiltrate and oximate the inside of the micropores, thereby increasing the adsorption rate and amount of gallium in the Bayer process solution of bauxite by the chelating resin, and effectively improving the analysis efficiency. It is particularly important to emphasize that the process of oximation of porous microspheres assisted by supercritical CO2 can not only effectively reduce the amount of reagents used, but also reduce the oximation reaction time from more than 10 hours to less than 5 hours, greatly shortening the production cycle and improving production efficiency. The microporous chelating resin under the technical solution of the present invention has a saturated adsorption capacity of 17 mg / L-20 mg / L for metallic gallium in the Bayer process circulating mother liquor, an effective resolution rate of more than 86%, and low-concentration gallium mother liquor will not affect the saturated adsorption capacity of the microporous chelating resin, and has significant social and economic benefits, and has important guiding significance and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The surface morphology of porous microspheres before and after supercritical CO2-assisted swelling is compared, where A is before supercritical CO2 swelling and B is after supercritical CO2 swelling;

[0026] Figure 2 The figure is a comparison of the morphology of porous microspheres assisted by supercritical CO2 amine oximation and porous microspheres assisted by traditional amine oximation, wherein A is the porous microspheres assisted by traditional amine oximation, and B is the porous microspheres assisted by supercritical CO2 amine oximation;

[0027] Figure 3This is the FT-IR spectrum of porous microspheres assisted by supercritical CO2 amine oximation;

[0028] Figure 4 The adsorption performance of supercritical CO2-assisted amine oximation porous microspheres on gallium in the Bayer process circulating mother liquor. DETAILED DESCRIPTION

[0029] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] Example 1

[0031] The present embodiment is improved for the preparation of chelating resin, and the specific operation steps of the preparation method of the improved chelating resin are as follows: (steps 1 to 4 are the preparation of porous microspheres, steps 5 to 6 are the amidoximation process of supercritical CO2-assisted swelling porous microspheres, and step 7 is the post-cleaning process, and the following parts are all by mass parts)

[0032] Step 1: First, add 30 parts of deionized water, 10 parts of CaCl2, 3 parts of NaCl, and then 2 parts of gelatin into the reactor by mass, stir slowly until the gelatin is fully dissolved, and then heat the reactor to 35-40°C.

[0033] Step 2: Add 20 parts of deionized water, 20 parts of acrylonitrile, 3 parts of hydroxyethyl methacrylate, 3 parts of divinylbenzene, 2 parts of hydroxyethyl acrylamide, 2.5 parts of toluene, 3.5 parts of aviation kerosene, 0.8 parts of benzoyl peroxide, and 0.2 parts of azobisisobutyronitrile into the batching kettle by mass, stir slowly and control the temperature at 45-50°C until all materials are fully dissolved.

[0034] Step 3: Pour all the materials in the batching kettle of step 2 into the reactor, heat the reaction system to 75±2°C, and keep the temperature for 2-3 hours; then heat it to 85±2°C, and keep the temperature for 2-3 hours; finally heat it to 95±2°C, and keep the temperature for 2-3 hours to complete the suspension polymerization.

[0035] Step 4: After the reaction is completed, the material obtained in step 3 is discharged, and then repeatedly washed with 30-40°C warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the beads are dried by air flow and sieved with a dryer at low temperature to obtain copolymer porous microspheres.

[0036] Step 5: Add porous microspheres to a supercritical CO2 reactor, seal the reactor, and introduce carbon dioxide, control the reactor pressure to 12-15Mpa, the temperature to 35-40°C, and the reaction time to 30 minutes. Supercritical CO2 is used to effectively swell the pore structure of the microspheres, so that the amine oximation reagent can infiltrate the spheres and react with amine oximation in the later stage.

[0037] Step 6: Supercritical CO2 assisted amine oximation of swollen porous microspheres. Take the swollen porous microspheres in step 5 and add them to the ingredients in a certain proportion, specifically 45 parts of beads, 20 parts of deionized water, 4 parts of ethanol, 13 parts of hydroxylamine sulfate, 5 parts of hydroxylamine hydrochloride, 10 parts of sodium hydroxide, and 3 parts of sodium carbonate, and stir for 10 minutes to make the materials uniform.

[0038] Then put the mixed materials into a supercritical CO2 reactor, seal the reactor, introduce carbon dioxide, control the reactor pressure to 12-15Mpa, temperature to 50-60℃, and reaction time to 3-4 hours to complete the amine oximation of the microspheres. After the reaction is completed, the temperature is lowered to below 30℃ before the material can be discharged.

[0039] Step 7: After the reaction is completed, discharge the material obtained in step 5, then wash it repeatedly with warm water at 30-40℃, and filter it with a filter with a filter to fully dissolve and remove the porogen. Finally, the product is dried by air flow and sieved at low temperature in a dryer to obtain a product of 20-50 mesh, and the amine-oximated porous microspheres are obtained. The use of supercritical CO2 technology can not only effectively reduce the swelling time of the porous microspheres, but also greatly reduce the amine-oximation reaction time of the porous microspheres. The modified adsorbent gallium microporous chelating resin obtained by this process has a saturated adsorption capacity of 19.02㎎ / L for metal gallium in the Bayer process circulating mother liquor, and the effective resolution rate reaches 84.46%.

[0040] Embodiment 2:

[0041] The present embodiment is improved at the preparation of chelating resin, and the preparation method of the improved chelating resin concrete operation steps are as follows:

[0042] Step 1: First, add 30 parts of deionized water, 10 parts of CaCl2, 2 parts of NaCl and 1 part of sodium nitrite into the reactor by mass, then add 3 parts of gelatin, 0.5 parts of polyvinyl alcohol and 0.5 parts of sodium carboxymethyl cellulose, stir slowly until the gelatin is fully dissolved, and then heat the reactor to 35-40°C.

[0043] Step 2: Add 20 parts of deionized water, 20 parts of acrylonitrile, 1 part of styrene, 1 part of butylated acrylamide, 3 parts of divinylbenzene, 2 parts of hydroxyethyl acrylamide, 2 parts of toluene, 3 parts of aviation kerosene, 0.5 parts of benzoyl peroxide, and 0.5 parts of azobisisobutyronitrile into a batching kettle, stir slowly and control the temperature at 45-50°C until all materials are fully dissolved.

[0044] Step 3: Pour all the materials in the batching kettle of step 2 into the reactor, heat the reaction system to 75±2℃, keep warm for 2-3 hours; then heat to 85℃±2℃, keep warm for 2-3 hours; finally heat to 95±2℃, keep warm for 2-3 hours. The suspension polymerization is completed.

[0045] Step 4: After the reaction is completed, the material obtained in step 3 is discharged, and then repeatedly washed with 30-40°C warm water, and filtered with a filter with a filter to fully dissolve and remove the porogen. Finally, the beads are dried by air flow and sieved with a dryer at low temperature to obtain copolymer porous microspheres.

[0046] Step 5: Add porous microspheres to a supercritical CO2 reactor, seal the reactor, and introduce carbon dioxide, control the reactor pressure to 12Mpa, the temperature to 35°C, and the reaction time to 45min. Supercritical CO2 is used to effectively swell the pore structure of the microspheres, so that the amine oximation reagent can infiltrate the spheres and react with amine oximation in the later stage.

[0047] Step 6: Supercritical CO2 assisted amine oximation of swollen porous microspheres. Take the swollen porous microspheres in step 5 and add them to the ingredients in a certain proportion. The specific proportion is 45 parts of bead mass, 20 parts of deionized water, 4 parts of ethanol; 12 parts of hydroxylamine sulfate, 6 parts of hydroxylamine hydrochloride, 10 parts of sodium hydroxide, and 3 parts of sodium carbonate. Stir for 10 minutes to make the materials uniform.

[0048] Then put the mixed materials into a supercritical CO2 reactor, seal the reactor, introduce carbon dioxide, control the reactor pressure to 12-15Mpa, temperature to 50-60℃, and reaction time to 3-4 hours to complete the amine oximation of the microspheres. After the reaction is completed, the temperature is lowered to below 30℃ before the material can be discharged.

[0049] Step 7: After the reaction is completed, discharge the material obtained in step 6, then wash it repeatedly with warm water at 30-40°C, and filter it with a filter with a screen to fully dissolve and remove the porogen. Finally, the product is dried by air flow and sieved at low temperature in a dryer to obtain 20-50 mesh products, thus obtaining oxime-treated porous microspheres. The use of supercritical CO2 technology can not only effectively reduce the swelling time of porous microspheres, but also greatly reduce the oxime reaction time of porous microspheres. After swelling with supercritical CO2, the surface of the sphere expands to a certain extent ( Figure 1Compared with the chelating resin of the traditional process, the chelating resin after supercritical CO2 solvent-assisted amine oximation has a higher surface area ( Figure 2 The surface of the modified gallium adsorbing microporous chelating resin obtained has a dense microporous structure, and the microspheres have abundant amine oxime groups that can effectively complex and adsorb gallium in the solution ( Figure 3 ), the resin has a fast adsorption rate for gallium, and the adsorption rate in 15 minutes is close to 84% ( Figure 4 ), after 45 minutes, the adsorption equilibrium was basically reached, and the adsorption rate was 87.34%; the saturated adsorption capacity of metallic gallium in the Bayer process circulating mother liquor reached 20.78 mg / L, and the effective resolution rate reached 86.22%.

[0050] Depend on Figure 1 It can be clearly seen that there are a lot of wrinkles on the surface of the porous microspheres before supercritical CO2 swelling, but after swelling, the surface of the microspheres becomes stretched and flat. This shows that the supercritical CO2 process can swell the porous microspheres very well, and this swelling is beneficial to the subsequent ammoximation reaction of the microspheres.

[0051] Depend on Figure 2 It can be clearly seen that the surface of the finished microspheres under the traditional ammoximation process is relatively flat, while the surface of the porous microspheres assisted by supercritical CO2 ammoximation has more wrinkles and a relatively large specific surface area. This shows that the supercritical CO2 process can well assist the ammoximation reaction of the swollen porous microspheres.

[0052] Supercritical CO2 has a high diffusivity and solubility, and this diffusion and dissolution are extremely beneficial to the swelling of the spherical resin. More importantly, by controlling the time, pressure and temperature of supercritical CO2, the degree of swelling can be monitored and controlled. The swelling process can achieve the ideal swelling degree without using any organic solvent, and related research has not been reported. Supercritical CO2 not only has a high diffusivity and solubility, but also, as a small molecule, the amine oximation reagent can also enter the pore structure of the microporous resin under the action of supercritical CO2. This diffusion and dissolution is beneficial to the amine oximation reaction of the amine oximation reagent on the surface of the sphere and the inside of the micropores, and greatly improves the adsorption efficiency and service life of the chelating resin.

[0053] In summary, in combination with the current production processes of chelating resins at home and abroad and the gallium recovery technology and process of chelating resins for Bayer process circulating mother liquor in the gallium recovery industry, the present invention provides a method for preparing a novel gallium adsorption porous chelating resin assisted by supercritical CO2 amine oximation. This process is not only easy to operate, but also can greatly improve the penetration of amine oximation reagents into spherical resins and amine oximation reactions, effectively improve the amine oximation degree of the resin, and then effectively improve the adsorption-desorption rate of gallium in the Bayer process circulating mother liquor by the chelating resin. What is particularly important is that the use of supercritical CO2 assisted process can effectively reduce the use of solvents, shorten the production cycle and improve production efficiency.

[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a novel gallium-adsorbing porous chelating resin assisted by supercritical CO2 amine oximation, characterized in that: The method comprises two parts: preparation of porous chelating resin beads and supercritical CO2-assisted amine oximation of the resin beads.

2. The method for preparing a novel gallium adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 1, characterized in that: The raw materials for preparing the porous chelating resin beads include, by weight, 5-20% of a main monomer, 1-5% of a modified monomer, 1-10% of a cross-linking monomer, 5-25% of a porogen, 0.5-5% of an initiator accounting for the total weight of the main monomer and the cross-linking monomer, 0.5-10% of a dispersant and 20-80% of salt water.

3. The method for preparing a novel gallium adsorbing porous chelating resin assisted by supercritical CO2 amine oximation according to claim 2, characterized in that: The salt water comprises one or two of calcium chloride, sodium chloride and sodium nitrite, and the purity thereof is above 99%. The dispersant comprises one or two of gelatin and polyvinyl alcohol.

4. The method for preparing a novel gallium adsorbing porous chelating resin assisted by supercritical CO2 amine oximation according to claim 2, characterized in that: The main monomer is acrylonitrile; the modified monomer is one or more of styrene, acrylic acid, methyl methacrylate, and hydroxyethyl methacrylate; the cross-linking monomer includes one or more of divinylbenzene, butylated acrylamide, N-butoxymethyl acrylamide, and hydroxyethyl acrylamide; the porogen includes one or more of toluene, paraffin, xylene, and aviation kerosene; and the initiator is one or a combination of benzoyl peroxide and azobisisobutyronitrile.

5. A method for preparing a novel gallium adsorbing porous chelating resin assisted by supercritical CO2 amine oximation according to claim 1 or 2, characterized in that: The preparation process of porous chelating resin specifically comprises the following steps: Step 1: First, add salt water in the reactor according to the ratio, then add a certain amount of dispersant, stir until the dispersant is completely dissolved, and then heat the reactor to the set temperature; Step 2: Add the main monomer, cross-linking monomer, modified monomer, porogen, and initiator into the reactor according to the ratio, control the stirring speed, increase the stirring speed after the materials are completely dissolved, and carry out suspension polymerization by step-by-step heating. After the reaction is completed, neutralize the solution after the reaction, filter the product, and finally dry the product with a mesh size below 60 in a dryer at low temperature, remove the porogen, wash the microspheres, and dry them to obtain porous microsphere beads; Step 3: Add the copolymeric porous microsphere beads obtained in step 2 to a supercritical CO2 reactor, and control the supercritical CO2 reaction temperature, time, and pressure to allow the pore structure of the microsphere to swell fully; Step 4: Add the swollen porous microsphere beads and the amine oxime reagent to the reaction medium in proportion, move the whole into the supercritical CO2 reactor after infiltration, control the supercritical CO2 reaction temperature, time and pressure, and after the reaction is completed, cool the reaction system to below 30°C and discharge the material; Step 5: Discharge the mixture obtained in step 4, filter out the solution with a filter, then wash the obtained product with water for multiple times, then filter and dry the water, and dry at low temperature to obtain the amine oxime porous microspheres.

6. The method for preparing a novel gallium adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 5, characterized in that: In step 2, the suspension polymerization is carried out by stage heating. Specifically, the temperature is raised to 75±2°C and kept warm for 2-3 hours; then the temperature is raised to 85±2°C and kept warm for 2-3 hours; finally, the temperature is raised to 95±2°C and kept warm for 2-3 hours.

7. The method for preparing a novel gallium adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 5, characterized in that: Step three is supercritical CO2-assisted swelling of porous microspheres. Effective swelling of porous microspheres can facilitate the subsequent infiltration of amine oxime reagents into the spheres and amine oxime reaction. The supercritical CO2-assisted swelling conditions of porous microspheres are 12-15Mpa, 30-45°C, and 30-60min.

8. The method for preparing a novel gallium-adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 5, characterized in that: Step four is the supercritical CO2-assisted swellable porous microspheres amine oximation process, the swollen porous microspheres are taken and added to the batching kettle in proportion, the mass fraction of the beads in the batching kettle is 35-55%, the reaction medium is one or two of water and ethanol, and the mass fraction of the reaction medium is 20-40%; the oximation reagent is one or two of hydroxylamine hydrochloride and hydroxylamine sulfate, and its mass fraction is 10-25%. After the whole system is soaked for 1 hour, it is moved into the supercritical CO2 reactor as a whole. The reaction conditions are 12Mpa-15Mpa, 50-60℃, 3-4 hours, and the amine oximation of the microspheres is completed.

9. The method for preparing a novel gallium-adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 5, characterized in that: In step 5, the obtained product is washed with water for multiple times until the pH value is 7, and the cleaning agent used is an aqueous solution of a mixture of sodium hydroxide and sodium carbonate with a mass fraction of 8%.

10. The method for preparing a novel gallium-adsorbing porous chelating resin by supercritical CO2-assisted amine oximation according to claim 5, characterized in that: In step 1, the main monomer and the cross-linking monomer must be deblocked with 5-10% sodium hydroxide solution before use.

Citation Information

Cited By

  • Method for selectively separating and extracting gallium

    CN120060672A

  • A method for selectively separating and extracting gallium

    CN120060672B

  • Amidoximated porous organic polymer as well as preparation method and application thereof

    CN120518858A

  • A porouso organic polymer of amidoxime and a preparation method and application thereof

    CN120518858B

  • Method for deeply separating and extracting gallium

    CN121513498A