Rubber reinforcing agent based on wollastonite and silica powder and preparation method thereof

By combining the treatment of rubber reinforcement based on wollastonite and silicon micropowder, coupled with coupling agent and dispersant, the problems of poor dispersion and environmental impact of traditional rubber reinforcement are solved, and the mechanical properties and wear resistance of rubber materials are significantly improved. Achieve environmentally friendly and efficient rubber reinforcement effect.

CN118956004APending Publication Date: 2024-11-15JIANGXI GUANGYUAN CHEM +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411155279.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional rubber reinforcement agents such as carbon black have dark colors, poor dispersion and unfriendly environment, which are difficult to meet the needs of modern industries for high-performance and environmentally friendly materials.

Method used

Using rubber reinforcement agent based on wollastonite and silicon micropowder, by optimizing particle size and component ratio, combining coupling agent and dispersant, ball milling and ultrasonic dispersion treatment are carried out to form a uniform rubber reinforcement powder and in the rubber matrix. Evenly disperse to improve mechanical properties.

Benefits of technology

It significantly improves the tensile strength, tear strength and wear resistance of rubber materials, avoids agglomeration, reduces production costs, complies with environmental protection regulations, and improves energy consumption and time efficiency during processing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of rubber reinforcing agents, in particular to a rubber reinforcing agent based on wollastonite and silica powder and a preparation method of the rubber reinforcing agent. The wollastonite composite material is prepared from the following raw materials in parts by weight: 25-45 parts of wollastonite powder, 10-30 parts of silica powder, 4-8 parts of a coupling agent, 2-3 parts of a dispersing agent and 3-6 parts of other auxiliaries. According to the rubber reinforcing agent based on the wollastonite and the silica powder and the preparation method of the rubber reinforcing agent, the prepared rubber reinforcing agent is environmentally friendly and efficient, and the requirement of the modern industry for high-performance rubber materials can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber reinforcing agents, and in particular to a rubber reinforcing agent based on wollastonite and silicon micropowder and a preparation method thereof. Background Art

[0002] Rubber materials are widely used in industrial production and daily life due to their unique elasticity and plasticity. However, the mechanical properties and wear resistance of pure rubber materials often cannot meet the requirements of specific application fields, so it is necessary to improve their performance by adding various rubber additives. Among the many rubber additives, rubber reinforcing agent is one of the key factors to improve the mechanical properties of rubber materials.

[0003] Traditional rubber reinforcing agents mostly use inorganic fillers such as carbon black and white carbon black. Although these materials can effectively improve the mechanical properties of rubber, they also have some disadvantages, such as dark color, poor dispersion, and environmental unfriendliness. With the increasingly stringent environmental regulations and the increasing demand for high-performance materials, the development of new, environmentally friendly and efficient rubber reinforcing agents has become an inevitable trend in the development of the industry.

[0004] Wollastonite and silica powder, as silicate minerals, have good mechanical properties and chemical stability, and are widely available and inexpensive. Their application in rubber can significantly improve the tensile strength, tear strength and wear resistance of rubber. Therefore, in order to solve the problems existing in the prior art, the present invention proposes a rubber reinforcing agent based on wollastonite and silica powder and a preparation method thereof. Summary of the invention

[0005] The invention provides a rubber reinforcing agent based on wollastonite and silicon micropowder and a preparation method thereof. The prepared rubber reinforcing agent is both environmentally friendly and highly efficient, and can meet the demand of modern industry for high-performance rubber materials.

[0006] The technical solution adopted by the present invention is: a rubber reinforcing agent based on wollastonite and silica powder, which is composed of the following raw materials in parts by weight: wollastonite powder accounts for 25-45 parts, silica powder accounts for 10-30 parts, coupling agent accounts for 4-8 parts, dispersant accounts for 2-3 parts, and other additives account for 3-6 parts.

[0007] As a further improvement of the present invention, the particle size of the wollastonite powder is 1-10 microns, and the particle size of the silicon micropowder is 0.1-1 microns.

[0008] As a further improvement of the present invention, the coupling agent is composed of a silane coupling agent and a titanate coupling agent, and the weight ratio of the silane coupling agent to the phthalate coupling agent is 3:1-2.

[0009] As a further improvement of the present invention, the dispersant is one or more of a polycarboxylate dispersant, a polyether dispersant, and a polyacrylate dispersant.

[0010] As a further improvement of the present invention, the other additives include antioxidants, anti-aging agents, plasticizers, and lubricants.

[0011] As a further improvement of the present invention, the antioxidant is one of 2,6-di-tert-butyl-p-cresol and 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; the antioxidant is one of N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N-(1-methylpropyl)-N'-phenyl-p-phenylenediamine; the plasticizer is one of dioctyl phthalate and diisobutyl phthalate; and the lubricant is one of stearic acid, paraffin, and polyethylene wax.

[0012] A method for preparing a rubber reinforcing agent based on wollastonite and silicon micropowder comprises the following steps:

[0013] Step 1: First, weigh wollastonite powder, silica powder, coupling agent, dispersant and other additives according to the above weight proportions;

[0014] Step 2: pre-treating the wollastonite powder and the silica powder so that the particle size of the wollastonite powder reaches between 1 and 10 microns, and the particle size of the silica powder reaches between 0.1 and 1 micron;

[0015] Step 3: Evenly mix the treated silica lime powder, silica powder, coupling agent, dispersant and other additives to ensure that each component is fully dispersed;

[0016] Step 4: ball milling and ultrasonic dispersion treatment of the uniformly mixed raw materials to further refine the particles and improve the mixing uniformity;

[0017] Step 5: adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 10-20% of the total weight of the mixed raw materials to form a uniform slurry;

[0018] Step 6: Drying the slurry by spray drying, freeze drying, or hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0019] Step 7: Screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent.

[0020] The invention discloses an application of a rubber reinforcing agent based on wollastonite and silicon micropowder. The rubber reinforcing agent is suitable for reinforcing natural rubber, styrene-butadiene rubber, nitrile rubber, chloroprene rubber, butyl rubber and EPDM rubber materials, and can significantly improve the tensile strength, tear strength and wear resistance of the rubber materials, so as to improve the processing performance of the rubber materials.

[0021] As a further improvement of the present invention, the application of the rubber reinforcing agent comprises the following steps:

[0022] S1: mixing the rubber reinforcing agent with the rubber matrix in a weight ratio of 2% to 6% to form a mixture;

[0023] S2: Use an open mixer or internal mixer to mix the mixture to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0024] S3: vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 140-180° C. and the vulcanization time is 10-30 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0025] S4: The obtained vulcanized rubber products are applied to the production of tires, belts, hoses, shoe materials, and shock absorber products to improve the quality and service life of the products.

[0026] The beneficial effect of the present invention is to provide an environmentally friendly and efficient rubber reinforcing agent, which can not only significantly improve the mechanical properties and wear resistance of rubber materials, but also has little impact on the environment during the production process. Specifically, the rubber reinforcing agent of the present invention has the following advantages:

[0027] (1) In the present invention, by adding wollastonite and silica powder, the rubber reinforcing agent performs well in improving the tensile strength, tear strength and wear resistance of the rubber material, so that the final rubber product has a longer service life and better performance.

[0028] (2) The optimized particle size of wollastonite powder and silica powder in the present invention ensures uniform dispersion of the rubber reinforcing agent in the rubber matrix, thereby avoiding the agglomeration phenomenon that may occur in traditional fillers and further improving the overall performance of the rubber product.

[0029] (3) The present invention significantly improves the compatibility and dispersibility of the rubber reinforcing agent in the rubber matrix by selecting appropriate coupling agents and dispersants, which helps to reduce the energy consumption and time cost of rubber products during processing.

[0030] (4) The rubber reinforcing agent preparation method of the present invention is simple, low-cost, and easy to mass-produce. The raw materials used are widely available and stable in price, which is conducive to reducing production costs. The rubber reinforcing agent does not contain harmful substances such as heavy metals, meets the requirements of current environmental protection laws and regulations, and is conducive to promoting the green and sustainable development of the rubber industry. DETAILED DESCRIPTION

[0031] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail in conjunction with the embodiments below. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0032] The present invention provides a rubber reinforcing agent based on wollastonite and silicon micropowder, characterized in that it is composed of the following raw materials in parts by weight: wollastonite powder accounts for 25-45 parts, silicon micropowder accounts for 10-30 parts, coupling agent accounts for 4-8 parts, dispersant accounts for 2-3 parts, and other additives account for 3-6 parts. The particle size of wollastonite powder is 1-10 microns, and the particle size of silicon micropowder is 0.1-1 microns. The coupling agent is composed of a silane coupling agent and a titanate coupling agent, and the weight ratio of the silane coupling agent to the phthalate coupling agent is 3:1-2. The dispersant adopts one or more of a polycarboxylate dispersant, a polyether dispersant, and a polyacrylate dispersant.

[0033] Other additives in the present invention include antioxidants, anti-aging agents, plasticizers, and lubricants. The antioxidant is selected from 2,6-di-tert-butyl-p-cresol and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; the anti-aging agent is selected from N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N-(1-methylpropyl)-N'-phenyl-p-phenylenediamine; the plasticizer is selected from dioctyl phthalate and diisobutyl phthalate; and the lubricant is selected from stearic acid, paraffin, and polyethylene wax.

[0034] A method for preparing a rubber reinforcing agent based on wollastonite and silica powder comprises the following steps: firstly weighing wollastonite powder, silica powder, coupling agent, dispersant and other auxiliary agents according to the above weight parts; pre-treating the wollastonite powder and silica powder so that the particle size of the wollastonite powder reaches between 1 and 10 microns, and the particle size of the silica powder reaches between 0.1 and 1 micron; then mixing the treated wollastonite powder, silica powder, coupling agent, dispersant and other auxiliary agents uniformly to ensure that each component is fully dispersed; ball milling and ultrasonic dispersion treatment of the uniformly mixed raw materials to further refine the particles and improve the mixing uniformity; adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 10-20% of the total weight of the mixed raw materials to form a uniform slurry; drying the slurry by spray drying, freeze drying and hot air drying to remove excess water to obtain dry rubber reinforcing agent powder; sieving the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent.

[0035] An application of a rubber reinforcing agent based on wollastonite and silicon micropowder, the rubber reinforcing agent is suitable for reinforcing natural rubber, styrene-butadiene rubber, nitrile rubber, chloroprene rubber, butyl rubber, and EPDM rubber materials, and can significantly improve the tensile strength, tear strength, and wear resistance of the rubber material to improve the processing performance of the rubber material. The application of the rubber reinforcing agent includes the following steps: mixing the rubber reinforcing agent with a rubber matrix at a weight ratio of 2%-6% to form a mixture; using an open mill and an internal mixer to mix the mixture to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix; vulcanizing the mixed rubber mixture, wherein the temperature during the vulcanization treatment is controlled at 140-180°C, and the vulcanization time is 10-30 minutes, to obtain a vulcanized rubber product with excellent physical properties; the obtained vulcanized rubber product is applied to the production of tires, tapes, hoses, shoe materials, and shock absorber products to improve the quality and service life of the products.

[0036] Embodiment 1:

[0037] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0038] (i) First, weigh 35 parts of wollastonite powder, 20 parts of silica powder, 4 parts of silane coupling agent, 2 parts of phthalate coupling agent, 2.5 parts of polycarboxylate dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of dioctyl phthalate, and 1 part of stearic acid;

[0039] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0040] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, dioctyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0041] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0042] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0043] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0044] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0045] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 4% by weight to form a mixture;

[0046] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0047] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 160° C. and the vulcanization time is 20 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0048] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0049] Embodiment 2:

[0050] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0051] (i) First, weigh 35 parts of wollastonite powder, 20 parts of silica powder, 4 parts of silane coupling agent, 2 parts of phthalate coupling agent, 2.5 parts of polycarboxylate dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of dioctyl phthalate, and 1 part of stearic acid;

[0052] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0053] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, dioctyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0054] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0055] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0056] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0057] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0058] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 5% by weight to form a mixture;

[0059] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0060] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization treatment is controlled at 150° C. and the vulcanization time is 25 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0061] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0062] Embodiment 3:

[0063] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0064] (i) First, weigh 35 parts of wollastonite powder, 20 parts of silica powder, 4 parts of silane coupling agent, 2 parts of phthalate coupling agent, 2.5 parts of polycarboxylate dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of dioctyl phthalate, and 1 part of stearic acid;

[0065] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0066] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, dioctyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0067] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0068] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0069] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0070] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0071] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 3% by weight to form a mixture;

[0072] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0073] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization treatment is controlled at 170° C. and the vulcanization time is 15 minutes, to obtain a vulcanized rubber product with excellent physical properties;

[0074] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0075] Embodiment 4:

[0076] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0077] (i) First, weigh 40 parts of wollastonite powder, 25 parts of silica powder, 4.5 parts of silane coupling agent, 2.5 parts of phthalate coupling agent, 3 parts of polycarboxylate dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of dioctyl phthalate, and 1 part of stearic acid;

[0078] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0079] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, dioctyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0080] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0081] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0082] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0083] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0084] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 4% by weight to form a mixture;

[0085] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0086] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 160° C. and the vulcanization time is 20 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0087] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0088] Embodiment 5:

[0089] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0090] (i) First, weigh 30 parts of wollastonite powder, 15 parts of silica powder, 3.5 parts of silane coupling agent, 1.5 parts of phthalate coupling agent, 2 parts of polycarboxylate dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of dioctyl phthalate, and 1 part of stearic acid;

[0091] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0092] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, dioctyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0093] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0094] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0095] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0096] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0097] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 4% by weight to form a mixture;

[0098] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0099] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 160° C. and the vulcanization time is 20 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0100] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0101] Embodiment 6:

[0102] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0103] (i) First, weigh 35 parts of wollastonite powder, 20 parts of silica powder, 4 parts of silane coupling agent, 2 parts of phthalate coupling agent, 2.5 parts of polyether dispersant, 1.5 parts of 2,6-di-tert-butyl-p-cresol, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of diisobutyl phthalate, and 1 part of polyethylene wax;

[0104] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0105] (iii) evenly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 2,6-di-tert-butyl-p-cresol, N-isopropyl-N'-phenyl-p-phenylenediamine, diisobutyl phthalate, and polyethylene wax to ensure that all components are fully dispersed;

[0106] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0107] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0108] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0109] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0110] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 4% by weight to form a mixture;

[0111] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0112] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 160° C. and the vulcanization time is 20 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0113] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0114] Embodiment 7:

[0115] This embodiment provides a preparation method and application of a rubber reinforcing agent based on wollastonite and silica powder, which specifically includes the following steps.

[0116] (i) First, weigh 35 parts of wollastonite powder, 20 parts of silica powder, 4 parts of silane coupling agent, 2 parts of phthalate coupling agent, 2.5 parts of polyether dispersant, 1.5 parts of 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 0.8 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 1.2 parts of diisobutyl phthalate, and 1 part of stearic acid;

[0117] (ii) pre-treating wollastonite powder and silica powder so that the particle size of wollastonite powder reaches between 5 microns and the particle size of silica powder reaches between 0.5 microns;

[0118] (iii) uniformly mixing the treated silica lime powder, silica powder, coupling agent, dispersant, 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, N-isopropyl-N'-phenyl-p-phenylenediamine, diisobutyl phthalate, and stearic acid to ensure that each component is fully dispersed;

[0119] (iv) subjecting the uniformly mixed raw materials to ball milling and ultrasonic dispersion treatment to further refine the particles and improve the mixing uniformity;

[0120] (5) adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 15% of the total weight of the mixed raw materials to form a uniform slurry;

[0121] (6) drying the slurry by hot air drying to remove excess water and obtain dry rubber reinforcing agent powder;

[0122] (7) screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent;

[0123] (8) mixing the rubber reinforcing agent with the rubber matrix in a ratio of 4% by weight to form a mixture;

[0124] (ix) Mixing the mixture using an internal mixer to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix;

[0125] (10) vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 160° C. and the vulcanization time is 20 minutes to obtain a vulcanized rubber product with excellent physical properties;

[0126] (XI) applying the obtained vulcanized rubber product to the production of tire products.

[0127] Performance Testing

[0128] The vulcanized rubber products prepared in the above Examples 1-7 were applied to the production of tire products, and the obtained tires were subjected to performance tests. At the same time, the rubber products prepared without adding rubber reinforcing agent were applied to the production of tire products, and the obtained tires were subjected to performance tests as a comparative example.

[0129] sample Tensile strength(MPa) Tear strength(N / mm) Example 1 23.34 85.64 Example 2 22.07 84.35 Example 3 22.48 83.89 Example 4 23.16 84.01 Example 5 23.29 85.27 Example 6 22.81 85.08 Example 7 22.67 84.52 Comparative Example 14.85 62.48

[0130] As can be seen from the above table, the vulcanized rubber products obtained by using the rubber reinforcing agent of the present invention are applied to the production of tire products, and the obtained tire products have significantly improved physical properties. Specifically, compared with the tire products without adding the rubber reinforcing agent, the tire products of Examples 1 to 7 show excellent performance in terms of tensile strength and tear strength. This shows that the rubber reinforcing agent of the present invention can effectively improve the mechanical properties of the rubber matrix, thereby enhancing the overall performance of the tire.

[0131] In summary, the rubber reinforcing agent of the present invention is both environmentally friendly and highly efficient, can meet the demand of modern industry for high-performance rubber materials, and has significant economic and environmental benefits in practical applications, and has broad market application prospects and promotion value.

[0132] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A rubber reinforcing agent based on wollastonite and silica powder, characterized in that: The invention is composed of the following raw materials in parts by weight: wollastonite powder accounts for 25-45 parts, silicon micropowder accounts for 10-30 parts, coupling agent accounts for 4-8 parts, dispersant accounts for 2-3 parts, and other auxiliary agents account for 3-6 parts.

2. A rubber reinforcing agent based on wollastonite and silicon powder according to claim 1, characterized in that: The particle size of the wollastonite powder is 1-10 microns, and the particle size of the silicon micropowder is 0.1-1 microns.

3. The rubber reinforcing agent based on wollastonite and silicon powder according to claim 1, characterized in that: The coupling agent consists of a silane coupling agent and a titanate coupling agent, and the weight ratio of the silane coupling agent to the phthalate coupling agent is 3:1-2.

4. The rubber reinforcing agent based on wollastonite and silicon powder according to claim 1, characterized in that: The dispersant is one or more of a polycarboxylate dispersant, a polyether dispersant, and a polyacrylate dispersant.

5. The rubber reinforcing agent based on wollastonite and silicon powder according to claim 1, characterized in that: The other additives include antioxidants, anti-aging agents, plasticizers, and lubricants.

6. The rubber reinforcing agent based on wollastonite and silicon powder according to claim 5, characterized in that: The antioxidant is one of 2,6-di-tert-butyl-p-cresol and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; the antioxidant is one of N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and N-(1-methylpropyl)-N'-phenyl-p-phenylenediamine; the plasticizer is one of dioctyl phthalate and diisobutyl phthalate; and the lubricant is one of stearic acid, paraffin and polyethylene wax.

7. A method for preparing a rubber reinforcing agent based on wollastonite and silicon powder, characterized in that: The following steps are involved: Step 1: First, weigh wollastonite powder, silica powder, coupling agent, dispersant and other additives according to the above weight proportions; Step 2: pre-treating the wollastonite powder and the silica powder so that the particle size of the wollastonite powder reaches between 1 and 10 microns, and the particle size of the silica powder reaches between 0.1 and 1 micron; Step 3: Evenly mix the treated silica lime powder, silica powder, coupling agent, dispersant and other additives to ensure that each component is fully dispersed; Step 4: ball milling and ultrasonic dispersion treatment of the uniformly mixed raw materials to further refine the particles and improve the mixing uniformity; Step 5: adding water to the mixed raw materials after ball milling and ultrasonic dispersion treatment, wherein the water accounts for 10-20% of the total weight of the mixed raw materials to form a uniform slurry; Step 6: Drying the slurry by spray drying, freeze drying, or hot air drying to remove excess water and obtain dry rubber reinforcing agent powder; Step 7: Screening the dried rubber reinforcing agent powder to obtain a finished rubber reinforcing agent.

8. An application of a rubber reinforcing agent based on wollastonite and silica powder, characterized in that: The rubber reinforcing agent is suitable for reinforcing natural rubber, styrene-butadiene rubber, nitrile rubber, chloroprene rubber, butyl rubber and EPDM rubber materials, and can significantly improve the tensile strength, tear strength and wear resistance of the rubber materials to improve the processing performance of the rubber materials.

9. The use of a rubber reinforcing agent based on wollastonite and silicon powder according to claim 8, characterized in that: The application of the rubber reinforcing agent comprises the following steps: S1: mixing the rubber reinforcing agent with the rubber matrix in a weight ratio of 2% to 6% to form a mixture; S2: Use an open mixer or internal mixer to mix the mixture to ensure that the rubber reinforcing agent is evenly dispersed in the rubber matrix; S3: vulcanizing the kneaded rubber mixture, wherein the temperature during the vulcanization is controlled at 140-180° C. and the vulcanization time is 10-30 minutes to obtain a vulcanized rubber product with excellent physical properties; S4: The obtained vulcanized rubber products are applied to the production of tires, belts, hoses, shoe materials, and shock absorber products to improve the quality and service life of the products.

Citation Information

Cited By

  • Silica micropowder composite powder and preparation method thereof

    CN119823594A

  • Heat-resistant coating based on modified silica powder and preparation method of heat-resistant coating

    CN120041008A