Thermosetting polyimide composite material and preparation and selective laser sintering molding method thereof

By combining thermoset polyimide composite materials with selective laser sintering molding method, the problem of low molding efficiency of polyimide parts in complex shapes is solved, and 3D printed parts with high temperature, high dimensional stability and excellent mechanical properties are achieved.

CN118956151APending Publication Date: 2024-11-15INST OF CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411196933.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art cannot achieve rapid 3D printing and forming of polyimide parts with high temperature resistance and high dimensional stability, especially the molding process of complex parts with complex shapes, long cycles and inefficient efficiency.

Method used

Provide a thermoset polyimide composite material, including polyimide resin prepolymer, reinforcement filler and flow aid, to achieve polyimide by a two-step reaction of laser sintering and thermal curing through selective laser sintering molding method High temperature and high dimensional stability of materials.

Benefits of technology

The excellent heat resistance, mechanical properties and dimensional stability of polyimide materials are achieved, with glass transition temperature ≥360℃, tensile strength ≥60MPa, and the X-direction linear shrinkage rate after curing is ≤6%, which improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956151A_ABST
    Figure CN118956151A_ABST
Patent Text Reader

Abstract

The invention relates to a thermosetting polyimide composite material as well as a preparation method and a selective laser sintering molding method thereof, belongs to 3D printing rapid molding, and solves the problem that 3D printing rapid molding of high-temperature-resistant and high-dimensional-stability polyimide parts cannot be realized. The composite material is prepared from the following components in parts by weight: 50 to 99 parts of polyimide resin prepolymer, 0.1 to 49.9 parts of reinforcing filler and 0.1 to 1 part of flow promoter, the sum of the parts by weight of the polyimide prepolymer, the reinforcing filler and the flow promoter is 100. The composite powder material is melted and pre-cured in the laser sintering process to form a self-supporting initial blank, and then the self-supporting initial blank is heated and thermally cured to obtain a polyimide composite material part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing rapid prototyping, and in particular to a thermosetting polyimide composite material and a preparation method and a selective laser sintering molding method thereof. Background Art

[0002] Selective Laser Sintering (SLS) is a 3D printing technology that selectively sintered powder materials through computer-controlled lasers, forming layer by layer, and quickly manufacturing three-dimensional solid components. Compared with 3D printing technologies such as fused deposition and digital light processing, SLS has the advantages of a wide range of molding materials, high material utilization, and no need for support, and has broad application prospects in the field of industrial manufacturing. At present, the materials suitable for SLS mainly include metal powders, ceramic precursor powders, and polymer powders. Among them, polymer materials are widely used in SLS molding due to their advantages such as low molding temperature, low required laser power, and difficulty in spheroidization. The polymer materials that have been used in SLS molding are mainly thermoplastic polymers and their composite materials, specifically covering polycarbonate, polystyrene, polyamide, polyetheretherketone, and polyimide. Compared with other SLS molding thermoplastic polymer materials, thermoplastic polyimide and polyetheretherketone have higher heat resistance, but it is still difficult to meet the application requirements of extreme high temperature environments in the industrial field.

[0003] As a special polymer material that can be used for a long time at a high temperature of 300°C, thermosetting polyimide is widely used in aerospace and rail transportation. However, at present, thermosetting polyimide is mainly prepared by hot molding and autoclave processes to prepare resin and composite parts. These traditional processes can only realize the molding and preparation of polyimide parts with simple shapes. For polyimide parts with complex shapes, they usually need to be split into multiple parts with simple shapes and structures, and then assembled into parts after being molded separately; or polyimide blocks, rods and plates are directly manufactured by subtractive manufacturing, and parts of the actual required size are obtained by cutting, drilling and grinding. This leads to complex molding processes, long cycles and low efficiency for polyimide parts with complex shapes. Summary of the invention

[0004] In view of the above analysis, the present invention aims to provide a thermosetting polyimide composite material and its preparation and selective laser sintering forming method, so as to solve the problem that the prior art cannot achieve 3D printing rapid prototyping of high temperature resistant and high dimensional stability polyimide parts.

[0005] The purpose of the present invention is mainly achieved through the following technical solutions:

[0006] In the first aspect, the present invention provides a thermosetting polyimide composite material for selective laser sintering, which comprises, by weight, 50 to 99 parts of a polyimide resin prepolymer, 0.1 to 49.9 parts of a reinforcing filler, and 0.1 to 1 part of a flow aid; the sum of the weight parts of the polyimide resin prepolymer, the reinforcing filler, and the flow aid is 100 parts.

[0007] Optionally, the thermosetting polyimide resin prepolymer has a structure of Formula I:

[0008]

[0009] Wherein, Ar is selected from at least one of the following groups:

[0010]

[0011] R1 is selected from at least one of the following groups:

[0012]

[0013] R2 is selected from at least one of the following groups:

[0014]

[0015] R3 is selected from at least one of the following groups:

[0016]

[0017] Optionally, the ratio of x to y is (95-60): (5-40), and the prepolymer design number average molecular weight M n It is 1000-5000g / mol.

[0018] Optionally, the composite material has a particle size of 10-100 μm.

[0019] Optionally, the flow aid includes one or more of silicon dioxide, titanium dioxide, aluminum oxide, and zinc oxide.

[0020] Optionally, the reinforcing filler includes one or more of carbon fiber powder, glass fiber powder, quartz fiber powder and aramid fiber powder.

[0021] In a second aspect, the present invention provides a method for preparing a thermosetting polyimide composite material, which is used to prepare the above-mentioned composite material, and is characterized in that it comprises the following steps:

[0022] (1) esterifying the aromatic dianhydride and the end-capping agent in an alcohol solvent to obtain an esterification solution;

[0023] (2) adding the esterification solution of step (1) into a suspension consisting of a rigid aromatic diamine, a flexible aromatic diamine and an alcohol solvent to react to obtain a thermosetting polyimide resin precursor solution;

[0024] (3) adding the reinforcing filler to the thermosetting polyimide resin precursor solution of step (2), stirring, and heating to complete imidization to obtain a thermosetting polyimide resin prepolymer containing the reinforcing filler;

[0025] (4) The thermosetting polyimide resin prepolymer containing reinforcing fillers in step (3) is crushed, a flow aid is added, mixed evenly, and sieved to obtain a composite powder material.

[0026] In a third aspect, the present invention provides a method for forming a thermosetting polyimide composite powder material, comprising the following steps:

[0027] (a) subjecting the composite material according to any one of claims 1 to 6 to laser sintering to obtain a self-supporting initial blank;

[0028] (b) The initial blank is heated to solidify, and then cooled to obtain a product.

[0029] Optionally, in step (b), the heating temperature is 375-385°C.

[0030] In a fourth aspect, the present invention provides an application of the above-mentioned thermosetting polyimide composite material in 3D printing.

[0031] In the fifth aspect, the present invention provides a part obtained by laser sintering of a thermosetting polyimide composite material, which is formed by the above-mentioned molding method. The part has excellent heat resistance, dimensional stability and mechanical properties, a glass transition temperature ≥360°C, a linear shrinkage rate in the X direction after curing ≤6%, and a tensile strength ≥60MPa.

[0032] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0033] (1) Selective laser sintering requires that the powder material has excellent powder fluidity and melt fluidity, while the existing pure thermosetting polyimide resin system cannot meet the above requirements. The present invention optimizes the composition system of the composite powder material so that the thermosetting polyimide resin material can meet the requirements of the SLS molding process, thereby making it possible to combine the thermosetting polyimide material with the SLS molding process. Specifically, the present invention selects the components of the composite material as thermosetting resin prepolymers (rather than thermoplastic polymer materials with high molecular weight) so that the composite material has excellent melt fluidity, exhibits low apparent viscosity during laser sintering, and is easy for molecular chains to diffuse and entangle; by adding a flow aid to the composite material, the fluidity of the composite powder material is significantly improved, which is beneficial to the spreading and leveling of the composite powder material during the SLS sintering process; by adding reinforcing fillers to the composite material, the mechanical properties of the final printed product are effectively improved.

[0034] (2) The existing SLS sintering method for thermoplastic polymers is a one-step molding process, during which only physical changes occur, but no chemical changes occur, that is, the performance of the molded product depends entirely on the performance of the material itself, and the heat resistance of the product is limited, which makes it difficult to meet the application requirements of extremely high temperature environments in the industrial field. The molding method of the present invention is a two-step molding process, namely a laser sintering process and a thermal curing process. During the laser sintering process, the thermosetting polyimide composite powder materials are prone to melting (physical change), accompanied by a cross-linking reaction of some end-capping groups (chemical change), forming a dense initial blank with self-supporting properties. In the subsequent temperature-raising thermal curing process (chemical change), the initial blank is dimensionally cured, and the end-capping groups of the thermosetting polyimide are completely cross-linked to obtain the final product. Therefore, the product obtained by laser sintering the thermosetting polyimide composite powder material provided by the present invention has excellent heat resistance and mechanical properties. Specifically, it is manifested as: glass transition temperature ≥360°C, and tensile strength ≥60MPa.

[0035] (3) The thermosetting polyimide composite powder material of the present invention undergoes melt pre-curing and curing reactions during the laser sintering process and the subsequent temperature-raising heat curing process, respectively. The molecular chains undergo diffusion entanglement, and the end-capping groups undergo cross-linking reactions. No external substances are involved in the physical and chemical processes involved, and no volatile products are generated. The dimensional stability of 3D printed parts is good. Specifically, the volume shrinkage after curing is low, and the linear shrinkage in the X direction is ≤6%.

[0036] (4) The present invention controls the proportion of each component in the composite material so that the composite powder material can meet the two-step molding requirements in the subsequent SLS molding process, causing corresponding physical and chemical changes, and ultimately obtaining a product with excellent heat resistance and mechanical properties and good dimensional stability.

[0037] (5) The present invention combines thermosetting polyimide materials with SLS molding technology, realizes 3D printing rapid prototyping of complex polyimide parts with high temperature resistance and high dimensional stability, and improves production efficiency.

[0038] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can be obvious from the description or understood by practicing the present invention.

[0039] The methods in the present invention are conventional methods unless otherwise specified. The raw materials can be obtained from commercial public channels or homemade in the laboratory unless otherwise specified. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0041] Figure 1 This is the stress-strain curve of the selective laser sintering thermosetting polyimide composite printed product in Example 13 of the present invention. DETAILED DESCRIPTION

[0042] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0043] The physical and chemical properties of thermosetting polyimide depend on the degree of curing of the resin. Thermosetting resin prepolymers have a much lower molecular weight than thermoplastic polymer materials, so they exhibit excellent melt fluidity, low apparent viscosity during laser sintering, and are easy for molecular chains to diffuse and entangle. As the degree of curing increases, the three-dimensional network structure of the resin is gradually formed, and the heat resistance and mechanical properties of the resin are improved. The characteristics of thermosetting polyimide make it possible to achieve the molding of self-supporting pre-cured initial blanks and final cured parts in sequence through the SLS-thermal curing two-step reaction molding process. It is urgent to explore technical methods that combine thermosetting polyimide materials and SLS molding to achieve rapid manufacturing of complex-shaped parts of polyimide materials and improve the temperature resistance level of SLS molded polymer parts.

[0044] In a first aspect, the present invention provides a thermosetting polyimide composite powder material for selective laser sintering, comprising a thermosetting polyimide resin prepolymer, a reinforcing filler and a flow aid.

[0045] Specifically, the thermosetting polyimide resin prepolymer has a structure of general formula I:

[0046]

[0047] Wherein, Ar is selected from at least one of the following groups:

[0048]

[0049] R1 is selected from at least one of the following groups:

[0050]

[0051] R2 is selected from at least one of the following groups:

[0052]

[0053] R3 is selected from at least one of the following groups:

[0054]

[0055] Among them, the ratio of x to y is (95-60):(5-40), for example, 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, 65:35, 60:40.

[0056] Prepolymer design number average molecular weight M n It is 1000-5000 g / mol, for example, 1000 g / mol, 1500 g / mol, 1679 g / mol, 2000 g / mol, 2300 g / mol, 2500 g / mol, 3000 g / mol, 3500 g / mol, 4000 g / mol, 4500 g / mol, 5000 g / mol.

[0057] The raw materials for preparing the thermosetting polyimide resin prepolymer include aromatic dianhydride, reactive end-capping agent, rigid aromatic diamine and flexible aromatic diamine.

[0058] The relationship between the above-mentioned reaction materials is as follows: when 2 molar equivalents of reactive end-capping agent are introduced, the amount of aromatic dianhydride added is 2-9.9 molar equivalents, and the amount of rigid aromatic diamine and flexible aromatic diamine added is 2.7-8.72 molar equivalents and 0.3-2.2 molar equivalents, respectively. In addition, the reaction system must meet the following molar ratio balance condition: 2 times the molar amount of aromatic dianhydride plus the molar amount of reactive end-capping agent is equal to 2 times the molar amount of rigid aromatic diamine plus 2 times the molar amount of flexible aromatic diamine, so as to ensure the stoichiometric balance between the reactants and achieve smooth reaction. At the same time, in order to regulate the heat resistance and processing properties of the product, the molar ratio of rigid aromatic diamine to flexible aromatic diamine should be in the range of 95:5 to 60:40.

[0059] Further, the aromatic dianhydride includes at least one of 2,3,3',4'-benzophenonetetracarboxylic dianhydride (a-BTDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (a-ODPA) and 4,4'-(hexafluoroisopropyl) diphthalic anhydride (6FDA).

[0060] Further, the reactive end-capping agent includes 4-(phenylprop-2-ynyl)phthalic anhydride, 4-(3-trifluoromethyl-1-phenylethynyl)phthalic anhydride, 4-phenylethynylphthalic anhydride (PEPA) and 4-phenylethynylphenoxyphthalic anhydride.

[0061] Further, the rigid aromatic diamine includes at least one of p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), 1,4-diamino-2-methylbenzene, 2,5-diaminotrifluorotoluene, 2,6-dimethylbenzene-1,4-diamine, 2,2'-dimethyl-4,4'-diaminobiphenyl and 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB).

[0062] Further, the flexible aromatic diamine includes at least one of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB), 1,3-bis(4'-aminophenoxy)benzene (1,3,4'-APB), 3,4'-diaminodiphenyl ether (3,4'-ODA) and 4,4'-diaminodiphenyl ether (4,4'-ODA), 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (6FAPB) and 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP).

[0063] It should be noted that the introduction of the flexible aromatic diamine structure can improve the melt fluidity of polyimide, making it easy for the thermosetting polyimide composite powder material to fuse during the laser sintering process to obtain a dense initial blank.

[0064] Specifically, the flow aid includes one or more of nano silicon dioxide, nano titanium dioxide, nano aluminum oxide, and nano zinc oxide.

[0065] It is worth noting that the experiment found that the special surface structure and thermodynamically unstable state of nanomaterials make it easy to move between powder materials, which can significantly improve the fluidity of composite powder materials and facilitate the coating and leveling of composite powder materials during SLS sintering. The flow aids selected in the present invention are all nanomaterials.

[0066] Specifically, the reinforcing filler includes one or more of micron-sized carbon fiber powder, micron-sized glass fiber powder, micron-sized quartz fiber powder and micron-sized aramid fiber powder. In the present invention, the introduction of micron-sized fiber powder can effectively improve the mechanical properties of the final printed product.

[0067] In the above embodiment, the composite powder material includes, by weight: 50 to 99 parts of polyimide resin prepolymer, 0.1 to 49.9 parts of reinforcing filler, and 0.1 to 1 part of flow aid, and the total weight of the polyimide prepolymer, reinforcing filler and flow aid is 100 parts.

[0068] Specifically, the polyimide resin prepolymer can be 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 92 parts, 95 parts, 97 parts, or 99 parts.

[0069] The reinforcing filler can be 0.1 parts, 0.5 parts, 0.8 parts, 1 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 47 parts, 49 parts, 49.9 parts.

[0070] The flow aid can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, or 1 part.

[0071] Compared with the prior art, the present invention optimizes the composition system of the composite powder material so that the thermosetting polyimide resin material can meet the requirements of the SLS molding process, thereby making it possible to combine the thermosetting polyimide material with the SLS molding process. The present invention controls the proportion of each component so that the composite powder material can meet the two-step molding requirements in the subsequent SLS molding process, and corresponding physical and chemical changes occur, ultimately obtaining a product with excellent heat resistance and mechanical properties and good dimensional stability.

[0072] In a second aspect, the present invention provides a method for preparing a thermosetting polyimide composite powder material for selective laser sintering, comprising the following steps:

[0073] (1) esterifying the aromatic dianhydride and the end-capping agent in an alcohol solvent of equal weight to obtain an esterification solution;

[0074] (2) adding the esterification solution to a suspension consisting of a rigid aromatic diamine, a flexible aromatic diamine and an alcohol solvent of equal weight to react and obtain a thermosetting polyimide resin precursor solution;

[0075] (3) adding a reinforcing filler to a thermosetting polyimide resin precursor solution, stirring, dispersing and mixing, and then heating to remove the solvent and complete imidization to obtain a thermosetting polyimide resin prepolymer containing a reinforcing filler;

[0076] (4) The thermosetting polyimide resin prepolymer containing reinforcing fillers is crushed, a flow aid is added, and the mixture is evenly mixed, and then sieved to obtain a composite powder material.

[0077] It is worth noting that adding the reinforcing filler to the thermosetting polyimide resin precursor solution and stirring and dispersing the mixture helps to coat the surface of the reinforcing filler with a layer of thermosetting polyimide prepolymer, thereby improving the interfacial bonding strength between the reinforcing filler and the thermosetting polyimide resin in the final printed product.

[0078] In step (4), the particle size of the composite powder material is in the range of 10-100 μm. If the particle size of the composite powder is too large, the thickness of the single layer of powder will increase, which will significantly increase the surface roughness of the 3D printed part; if the particle size of the composite powder is too small, the powder is prone to generate static electricity, making it difficult to spread the powder.

[0079] In a third aspect, the present invention also provides a method for forming a thermosetting polyimide composite powder material for selective laser sintering, comprising the following steps:

[0080] (a) subjecting the thermosetting polyimide composite powder material to laser sintering layer by layer to melt and pre-solidify to obtain a self-supporting initial blank;

[0081] (b) The initial blank is heated and solidified, and then cooled to below 200° C. by natural cooling to obtain a product.

[0082] In step (a), the thermosetting polyimide composite powder materials are easily fused together, accompanied by a cross-linking reaction of some end-capping groups, to form a dense initial blank with self-supporting properties. The specific sintering process parameters are as follows:

[0083] Sintering power: 4-6W, for example, 4W, 4.5W, 5W, 5.5W, 6W;

[0084] Laser scanning speed 350-450 mm / s, for example, 350 mm / s, 370 mm / s, 390 mm / s, 400 mm / s, 420 mm / s, 450 mm / s;

[0085] The thickness of a single layer is 0.05-0.2 mm, for example, 0.05 mm, 0.1 mm, 0.15 mm, 0.2 mm;

[0086] The scanning interval is 0.1-0.2 mm, for example, 0.1 mm, 0.12 mm, 0.14 mm, 0.16 mm, 0.18 mm, 0.2 mm.

[0087] The present invention controls the sintering process parameters within the above range, so that the composite powder material can be melted (physical change) and pre-solidified (chemical change), thereby obtaining a dense initial blank with self-supporting properties.

[0088] In step (b), the heating temperature is 375-385°C, for example, 375°C, 378°C, 380°C, 382°C, 385°C.

[0089] It should be noted that the heating process in step (b) is a gradient heating process, that is, in the process of heating from room temperature to 375-385°C, a constant temperature step is set at one or several temperatures, and the constant temperature time of each constant temperature step is 1-2h, for example, 1h, 1.5h, 2h.

[0090] Specifically, the temperature of the constant temperature step is set to one or more of 250°C, 270°C, 290°C, 300°C, 320°C, 340°C, 360°C and 380°C.

[0091] The present invention can realize the dimensional solidification of the initial blank by adopting the gradient temperature increase in step (b), and the end-capping groups of the thermosetting polyimide are completely cross-linked to obtain the final product.

[0092] Example 1

[0093] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 22.31 g (0.0692 mol) of 2,3,3',4'-benzophenone tetracarboxylic dianhydride (a-BTDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 17.02 g (0.0616 mol) of 4-(phenylprop-2-ynyl)phthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0094] 24.64g of micron-grade carbon fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler was crushed, 0.11g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 45:54.8:0.2).

[0095] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 350mm / s; scanning spacing is 0.16mm; single layer thickness is 0.15mm.

[0096] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0097] Example 2

[0098] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.27 g (0.0908 mol) of 2,3,3',4'-benzophenone tetracarboxylic dianhydride (a-BTDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 4.57 g (0.0184 mol) of 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.77 g (0.0800 mol) of 2-methyl-p-phenylenediamine and 5.85 g (0.0200 mol) of 1,3-bis(4'-aminophenoxy)benzene (1,3,4'-APB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0099] 7.51g of micron-grade glass fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.04g of nano titanium dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 20:79.9:0.1).

[0100] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 5W; scanning rate is 390mm / s; scanning spacing is 0.2mm; single layer thickness is 0.05mm.

[0101] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 385℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0102] Example 3

[0103] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 26.85 g (0.0833 mol) of 2,3,3',4'-benzophenone tetracarboxylic dianhydride (a-BTDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 9.23 g (0.0334 mol) of 4-(phenylprop-2-ynyl)phthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 10.21 g (0.0750 mol) of 2,6-dimethylbenzene-1,4-diamine and 10.71 g (0.0250 mol) of 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (6FAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0104] 10.04g of micron-sized carbon fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler was crushed, 0.12g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid was 25:74.7:0.3).

[0105] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 370mm / s; scanning spacing is 0.16mm; single layer thickness is 0.1mm.

[0106] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320o C / 1h, 340℃ / 1h, 360℃ / 1h, 382℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0107] Example 4

[0108] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 23.71 g (0.0806 mol) of 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 9.64 g (0.0388 mol) of 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 22.42 g (0.0700 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB) and 6.01 g (0.0300 mol) of 3,4'-diaminodiphenyl ether (3,4'-ODA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0109] 1.58g of micron-grade quartz fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.10g of nano-alumina flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 5:94.7:0.3).

[0110] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 6W; scanning rate is 420mm / s; scanning spacing is 0.12mm; single layer thickness is 0.1mm.

[0111] The sintered blank is placed in a high temperature oven for curing. The curing process is 250℃ / 2h, 270℃ / 2h, 290 o C / 2h, 300℃ / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0112] Example 5

[0113] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 26.15 g (0.0889 mol) of 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 7.56 g (0.0222 mol) of 4-phenylethynylphenoxyphthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 10.90 g (0.0800 mol) of 2,6-dimethylbenzene-1,4-diamine and 7.37 g (0.0200 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0114] 12.89g of micron-grade aramid fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler was crushed, 0.09g of nano zinc oxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid was 30:69.8:0.2).

[0115] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0116] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 378℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0117] Example 6

[0118] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 19.61 g (0.0667 mol) of 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 21.06 g (0.0666 mol) of 4-(3-trifluoromethyl-1-phenylethynyl)phthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 15.85 g (0.0900 mol) of 2,5-diaminotrifluorotoluene and 2.00 g (0.0100 mol) of 3,4'-diaminodiphenyl ether (3,4'-ODA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0119] 10.03g of micron-grade glass fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.08g of nano titanium dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 25:74.8:0.2).

[0120] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 450mm / s; scanning spacing is 0.1mm; single layer thickness is 0.1mm.

[0121] The sintered blank is placed in a high temperature oven for curing. The curing process is 270℃ / 2h, 290℃ / 2h, 300℃ / 2h. o C / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0122] Example 7

[0123] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 23.07 g (0.0744 mol) of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (a-ODPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 12.71 g (0.0512 mol) of 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 30.42 g (0.0950 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB) and 1.46 g (0.0050 mol) of 1,3-bis(4'-aminophenoxy)benzene (1,3,4'-APB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0124] 20.17g of micron-sized carbon fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.25g of nano-silicon dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 40:59.5:0.5).

[0125] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 350mm / s; scanning spacing is 0.1mm; single layer thickness is 0.2mm.

[0126] The sintered blank is placed in a high temperature oven for curing. The curing process is 270℃ / 2h, 290℃ / 2h, 300℃ / 2h. oC / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 375℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0127] Example 8

[0128] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 24.13 g (0.0778 mol) of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (a-ODPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 11.03 g (0.0444 mol) of 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 11.00 g (0.0900 mol) of 2-methyl-p-phenylenediamine and 2.00 g (0.0100 mol) of 3,4'-diaminodiphenyl ether (3,4'-ODA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0129] 3.35g of micron-grade quartz fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.12g of nano-silicon dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 10:89.65:0.35).

[0130] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 5.5W; scanning rate is 400mm / s; scanning spacing is 0.1mm; single layer thickness is 0.1mm.

[0131] The sintered blank is placed in a high temperature oven for curing. The curing process is 270℃ / 2h, 290℃ / 2h, 300℃ / 2h. o C / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 378℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0132] Example 9

[0133] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 24.82 g (0.0800 mol) of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (a-ODPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 13.61 g (0.0400 mol) of 4-phenylethynylphenoxyphthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 19.11 g (0.0900 mol) of 2,2'-dimethyl-4,4'-diaminobiphenyl and 2.92 g (0.0100 mol) of 1,3-bis(4'-aminophenoxy)benzene (1,3,4'-APB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0134] 5.30g of micron-sized carbon fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler was crushed, 0.04g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid was 15:84.9:0.1).

[0135] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 5W; scanning rate is 370mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0136] The sintered blank is placed in a high temperature oven for curing. The curing process is 270℃ / 2h, 290℃ / 2h, 300℃ / 2h. o C / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 385℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0137] Example 10

[0138] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 33.32 g (0.0750 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 h to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 13.81 g (0.0500 mol) 4-(phenylprop-2-ynyl) phthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 h to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 8.65 g (0.0800 mol) of m-phenylenediamine (m-PDA) and 4.00 g (0.0200 mol) of 4,4'-diaminodiphenyl ether (4,4'-ODA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0139] 16.23g of micron-grade quartz fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.14g of nano-silicon dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 35:64.7:0.3).

[0140] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.15mm.

[0141] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 382℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0142] Embodiment 11

[0143] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 33.32 g (0.0750 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 12.41 g (0.0500 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 27.22 g (0.0850 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB) and 7.78 g (0.0150 mol) of 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0144] 7.52g of micron-grade glass fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.08g of nano titanium dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 20:79.8:0.2).

[0145] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.12mm; single layer thickness is 0.1mm.

[0146] The sintered blank is placed in a high temperature oven for curing. The curing process is 270℃ / 2h, 290℃ / 2h, 300℃ / 2h. oC / 2h, 320℃ / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0147] Example 12

[0148] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 36.35 g (0.0818 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 11.50 g (0.0364 mol) 4-(3-trifluoromethyl-1-phenylethynyl) phthalic anhydride and an equal amount of anhydrous ethanol were added, and the mixture was heated and stirred to clarify, and then refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 8.17 g (0.0600 mol) of 2,6-dimethylbenzene-1,4-diamine and 8.01 g (0.0400 mol) of 3,4'-diaminodiphenyl ether (3,4'-ODA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0149] 30.24g of micron-grade glass fiber powder and carbon fiber powder mixed reinforcing filler are added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.24g of nano titanium dioxide and silicon dioxide mixed flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 50:49.6:0.4).

[0150] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam is scanned. This is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4W; scanning rate is 390mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0151] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0152] Embodiment 13

[0153] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0154] 12.89g of micron-sized carbon fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.09g of nano-silicon dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 30:69.8:0.2).

[0155] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0156] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0157] Comparative Example 1

[0158] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 10.81 g (0.1000 mol) of p-phenylenediamine (p-PDA) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask. Under nitrogen protection, the mixture was heated and stirred until the diamine was completely dissolved. The reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0159] 12.89g of micron-sized carbon fiber powder was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing fillers. After the thermosetting polyimide resin prepolymer containing reinforcing fillers was crushed, 0.09g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing fillers, polyimide prepolymer and flow aid was 30:69.8:0.2).

[0160] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0161] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0162] Comparative Example 2

[0163] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0164] 12.86g of micron-sized carbon fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. Then, the composite powder material with a particle size range of 10-100μm was obtained by crushing and screening (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 30:70:0). Its main properties are shown in Table 1.

[0165] Comparative Example 3

[0166] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0167] 60.00g of thermosetting polyimide resin precursor solution was subjected to stepwise temperature treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h to remove the solvent and complete imidization to obtain a thermosetting polyimide resin prepolymer containing reinforcing fillers. Then 0.06g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid was 0:99.8:0.2).

[0168] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0169] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 o C / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0170] Comparative Example 4

[0171] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0172] 12.89g of micron-sized carbon fiber powder reinforcing filler is added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution is obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent is removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization is completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler is crushed, 0.09g of nano-silicon dioxide flow aid is added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid is 30:69.8:0.2).

[0173] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0174] The sintered green sheet was placed in a high temperature oven for curing. The curing process was to directly heat the temperature to 380°C / 1h and then cool it down to obtain the final product. The main properties of the product are shown in Table 1.

[0175] Comparative Example 5

[0176] In a three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 29.62 g (0.0667 mol) (hexafluoroisopropyl) diphthalic anhydride (6FDA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In another three-necked round-bottom flask equipped with a mechanical stirrer and a spherical reflux condenser, 16.53 g (0.0666 mol) 4-phenylethynylphthalic anhydride (PEPA) and an equal amount of anhydrous ethanol were added, and the mixture was heated, stirred, clarified, and refluxed for 4 hours to obtain a homogeneous esterification solution. In a three-necked round-bottom flask equipped with a mechanical stirrer, a spherical reflux condenser and a nitrogen inlet and outlet, 9.73 g (0.0900 mol) of p-phenylenediamine (p-PDA) and 3.68 g (0.0100 mol) of 4,4-bis(3'-aminophenoxy)biphenyl (m-BAPB) and an equal mass of anhydrous ethanol were added, and then the two esterification solutions obtained above were mixed and added to the above three-necked flask, and heated and stirred under nitrogen protection until the diamine was completely dissolved, and the reaction was continued to stir at room temperature for 12 hours to obtain a thermosetting polyimide resin precursor solution.

[0177] 47.37g of micron-sized carbon fiber powder reinforcing filler was added to 60.00g of thermosetting polyimide resin precursor solution, and a mixed solution was obtained by magnetic stirring and ultrasonic dispersion. Then, the solvent was removed by step-heating treatment at 120℃ / 2h, 150℃ / 1h, 180℃ / 1h, 200℃ / 2h, and 250℃ / 2h, and imidization was completed to obtain a thermosetting polyimide resin prepolymer containing reinforcing filler. After the thermosetting polyimide resin prepolymer containing reinforcing filler was crushed, 1.58g of nano-silicon dioxide flow aid was added and mixed evenly, and then sieved to obtain a composite powder material with a particle size range of 10-100μm (the weight ratio of reinforcing filler, polyimide prepolymer and flow aid was 60:38:2).

[0178] The thermosetting polyimide composite powder material is added to the powder bed of the selective laser sintering equipment, and the powder material is evenly spread using a scraper. The laser emits laser along a preset path according to the two-dimensional pattern on the computer. After laser scanning, the surface of the powder melts, and then the workbench is moved down by one layer thickness and the powder is spread again, and the laser beam scans, and this is repeated to obtain a laser sintered blank. The selective laser sintering molding process parameters are as follows: laser power is 4.5W; scanning rate is 400mm / s; scanning spacing is 0.14mm; single layer thickness is 0.1mm.

[0179] The sintered blank is placed in a high temperature oven for curing. The curing process is 290℃ / 2h, 300℃ / 2h, 320 oC / 1h, 340℃ / 1h, 360℃ / 1h, 380℃ / 1h, and then cooled to obtain the final product. Its main properties are shown in Table 1.

[0180] Table 1. Summary of the formula of thermosetting polyimide composite powder materials for SLS and the properties of printed parts

[0181]

[0182] It can be seen from Table 1 that the T values ​​of the thermosetting polyimide composite materials in Examples 1-13 of the present invention are g The temperature is 362.1-411.5°C, the tensile strength of the printed strip is 60.1-81.0 MPa, and the dimensional shrinkage (linear shrinkage in the X direction) is 3.7-5.9%.

[0183] The molecular weight of the thermosetting polyimide resin matrix in Example 13, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 is basically the same. The difference between the six polyimides is that the main chain structure of the thermosetting polyimide in Example 13 is a rigid and flexible structure; no flexible structure is introduced into the main chain of the thermosetting polyimide molecule in Comparative Example 1, and the molecular chain exhibits high rigidity; no flow aid is added in Comparative Example 2; no reinforcing filler is added in Comparative Example 3; Comparative Example 4 does not adopt a gradient temperature rise curing method and the dosage ratio of the polyimide resin prepolymer, reinforcing filler and flow aid in Comparative Example 5 is not within an appropriate range. The six thermosetting polyimide composite powder materials exhibit different properties due to different main chain structures and formulations. As can be seen from Table 1, the mechanical properties of the thermosetting polyimide composite powder material in Example 13 are significantly higher than those in Comparative Example 1. The reason is that the introduction of the flexible structure in Example 13 can reduce the melt viscosity of the resin prepolymer, which is beneficial to the powder melting of the resin during the laser sintering and curing process, and the printed parts have high density and improved mechanical properties. In Comparative Example 2, the thermosetting polyimide composite powder material did not add a flow aid. Due to the electrostatic effect between the powders, the composite powder material had poor fluidity, and the powder could not be spread and scraped during the sintering process, and the sample strips could not be successfully printed. In Comparative Example 3, the thermosetting polyimide composite powder material did not add reinforcing fillers, and the mechanical properties of the printed parts were much lower than those of Example 13, and there was obvious dimensional shrinkage. Comparative Example 4 used a direct heating method, and there were a large number of pores inside the final product, with low mechanical properties and high dimensional shrinkage. Comparative Example 5 had a high melt viscosity of the composite material and low mechanical strength of the printed sample strips due to excessive addition of reinforcing fillers and flow aids.

[0184] The above performance comparison fully demonstrates that the rigid structure and the flexible structure exist simultaneously in the molecular main chain structure, and the addition of reinforcing fillers and flow aids can give the selective laser sintering thermosetting polyimide composite material products the best comprehensive performance. The excellent comprehensive performance of the thermosetting polyimide composite powder materials in Examples 1-13 is a manifestation of the beneficial effects of the present invention compared with the prior art.

[0185] Figure 1 The stress-strain curve of the selective laser sintering thermosetting polyimide composite printed product in Example 13. Thanks to the excellent melt fluidity of the thermosetting polyimide prepolymer, the thermosetting polyimide composite powder materials are easily melted during the laser sintering process, accompanied by the cross-linking reaction of some end-capping groups, forming a self-supporting dense initial blank. In the subsequent gradient heating process, the initial blank is solidified, and the end-capping groups of the thermosetting polyimide are completely cross-linked, so the printed product exhibits high mechanical properties and heat resistance.

[0186] It should be noted that by replacing dianhydride, diamine, end-capping agent, reinforcing filler, and flow aid with substances other than those in Examples 1-13, or replacing the dosage of the substances and the process conditions with dosages or process conditions other than those in Examples 1-13, the performance of the obtained parts is similar to that of Examples 1-13, and they are not listed one by one here.

[0187] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A thermosetting polyimide composite material, characterized in that: In parts by weight, it comprises 50 to 99 parts of polyimide resin prepolymer, 0.1 to 49.9 parts of reinforcing filler, and 0.1 to 1 part of flow aid; The total weight of the polyimide resin prepolymer, the reinforcing filler and the flow aid is 100 parts.

2. The composite material according to claim 1, characterized in that The thermosetting polyimide resin prepolymer has the structure of general formula I: Wherein, Ar is selected from at least one of the following groups: R1 is selected from at least one of the following groups: R2 is selected from at least one of the following groups: R3 is selected from at least one of the following groups:

3. The composite material according to claim 2, characterized in that The ratio of x to y is (95-60): (5-40), and the prepolymer design number average molecular weight M n It is 1000-5000g / mol.

4. The composite material according to claim 1, characterized in that The particle size of the composite material is 10-100 μm.

5. The composite material according to claim 1, characterized in that The flow aid includes one or more of silicon dioxide, titanium dioxide, aluminum oxide and zinc oxide.

6. The composite material according to claim 1, characterized in that The reinforcing filler includes one or more of carbon fiber powder, glass fiber powder, quartz fiber powder and aramid fiber powder.

7. A method for preparing a thermosetting polyimide composite material, characterized in that: Used to prepare the composite material according to any one of claims 1 to 6, characterized in that it comprises the following steps: (1) esterifying the aromatic dianhydride and the end-capping agent in an alcohol solvent to obtain an esterification solution; (2) adding the esterification solution of step (1) into a suspension consisting of a rigid aromatic diamine, a flexible aromatic diamine and an alcohol solvent to react to obtain a thermosetting polyimide resin precursor solution; (3) adding the reinforcing filler to the thermosetting polyimide resin precursor solution of step (2), stirring, and heating to complete imidization to obtain a thermosetting polyimide resin prepolymer containing the reinforcing filler; (4) The thermosetting polyimide resin prepolymer containing reinforcing fillers in step (3) is crushed, a flow aid is added, mixed evenly, and sieved to obtain a composite material.

8. A method for molding a thermosetting polyimide composite powder material, characterized in that: The steps include: (a) subjecting the composite material according to any one of claims 1 to 6 to laser sintering to obtain a self-supporting initial blank; (b) The initial blank is heated to solidify, and then cooled to obtain a product.

9. Use of the composite material according to any one of claims 1 to 6 in 3D printing.

10. A part obtained by laser sintering of a thermosetting polyimide composite material, characterized in that: The product is obtained by molding using the molding method of claim 8, and has excellent heat resistance, dimensional stability and mechanical properties, a glass transition temperature of ≥360°C, a linear shrinkage in the X direction after curing of ≤6%, and a tensile strength of ≥60MPa.

Citation Information

Cited By

  • Thermosetting polyimide resin, workpiece, preparation method, forming method and application

    CN119823379A