Steel slag conversion method for removing total chromium
By controlling the reaction conditions, the steel slag is converted into carboxy modified powders loaded with hydroxyapatite, and the reduction of Cr(VI) and adsorption and fixation of Cr(III) is achieved by controlling the reaction conditions, which solves the chromium contamination in the prior art. The problem has reduced costs and improved efficiency, and achieved efficient utilization of steel slag solid waste.
Patent Information
- Application Number
- CN202410893387.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The prior art is difficult to effectively remove chromium in the Cr(VI)-containing wastewater, and the reduced Cr(III) may be oxidized to Cr(VI) in the natural environment, resulting in environmental pollution, and the resource utilization method of steel slag is costly. And inefficient.
By controlling the reaction conditions, the steel slag is ground into powder, and the water bath is treated with organic carboxylic acid in a mixed solvent of alcohol and water to form a carboxylic group-modified steel slag powder, and phosphate is added to an alkaline environment for water bath reaction to prepare a load The carboxy modified steel slag powder of hydroxyapatite is used to reduce Cr(VI) and adsorption and fixation of Cr(III) products under visible light irradiation.
The total chromium removal in sewage is achieved, cost reduction, efficiency improvement, good repeatability, simple operation, and effective reuse of steel slag solid waste.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention relates to a steel slag conversion method for removing total chromium, and belongs to the field of functional materials. Technical Background
[0002] Wastewater used in metallurgy, electroplating, leather and other industries contains a large amount of Cr(VI) ions, which are harmful to humans. Cr(VI) is significantly toxic. Frequent exposure to Cr(VI) can cause cancer in body tissues and organs. When the concentration of Cr(VI) is too high, it can even lead to death. It is crucial to eliminate Cr(VI) in wastewater, but if the reduced Cr(III) product is not removed in time, especially in the natural environment, it will be reoxidized by manganese oxides and other substances and turned back into Cr(VI), which will continue to harm the environment. Therefore, after Cr(VI) is reduced to Cr(III), continuing to adsorb and fix Cr(III) to achieve total chromium removal is an effective way to solve the above problems. Industrial by-products represented by steel slag are a type of solid waste with the largest emission volume, and its resource utilization is one of the current research hotspots. Efficient utilization of solid waste can be achieved by converting steel slag into efficient chromium removal materials.
[0003] In the present invention, by controlling the reaction conditions, the rich elements such as Fe and Ca in the steel slag can be effectively utilized, the iron ions in the steel slag are converted into carboxylic acid complexes, and the calcium ions are converted into calcium hydroxyphosphate, thereby respectively realizing the light reduction of Cr(VI) and the adsorption and fixation of Cr(III) products, thereby achieving the purpose of effective chromium removal. Summary of the invention
[0004] The purpose of the present invention is to provide a steel slag conversion method for total chromium removal, which effectively utilizes steel slag solid waste, is simple, is conducive to batch preparation, can greatly reduce costs, improve efficiency, and has great practical application significance.
[0005] The present invention aims to achieve functional transformation of steel slag by simple reaction parameter control, so as to reduce costs and realize batch synthesis.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] The present invention provides a steel slag conversion method for total chromium removal, characterized in that it comprises the following steps:
[0008] (1) First, the steel slag is ground into 30-200 mesh and sieved. The obtained powder is treated with an organic carboxylic acid in a mixed solvent of alcohol and water in a water bath at a temperature of 50-90° C. for 1-10 hours to obtain a carboxyl-modified steel slag powder, wherein the carboxyl group is complexed with Fe ions on the surface;
[0009] (2) dispersing the powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=8-11), and then adding phosphate to heat the reaction in a water bath at a temperature of 60-90° C. for 5-10 hours to obtain a carboxyl-modified steel slag powder loaded with hydroxyapatite.
[0010] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 60 mesh; the dosage relationship of steel slag powder: organic carboxylic acid: alcohol and water is (2-5) g: 20-40 mL: (2-8) mL: (20-40) mL.
[0011] The alcohol is ethanol, ethylene glycol, glycerol, preferably ethanol; the organic carboxylic acid is formic acid, acetic acid, propionic acid, butyric acid, valeric acid, preferably acetic acid;
[0012] Wherein, in step (2), the suspension is adjusted to pH=8-11 by adding ammonia water.
[0013] The phosphate is diammonium hydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, diammonium hydrogen phosphate, preferably diammonium hydrogen phosphate; the mass ratio of the organic carboxylic acid modified steel slag to the phosphate is 7-10:1, preferably 9-10:1.
[0014] The prepared carboxyl modified steel slag powder loaded with hydroxyapatite can realize Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, that is, it can realize Cr(VI) reduction to Cr(III) under visible light irradiation, and at the same time adsorb and fix the obtained Cr(III) products, so that the total chromium in the solution is reduced; wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.4-0.6 mg / L; the Cr(VI) concentration in the solution is 2-20 mg / L, preferably 5-15 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: ≤0.1 mg / L, and the total chromium Cr concentration is: ≤1 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0015] The beneficial effects of the present invention are as follows: the preparation method of the present invention can effectively convert Fe and Ca elements in steel slag into chromium removal materials, can achieve total chromium removal in sewage, has good repeatability, simple operation, low cost, and effectively realizes the recycling of steel slag solid waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 : UV-visible absorption spectra of steel slag, steel slag modified by organic carboxylic acid in step (1) and steel slag modified by phosphate in step (2);
[0017] Figure 2 : Changes in the UV-visible absorption spectrum of Cr(VI) in an aqueous solution containing Cr(VI) under visible light irradiation under the action of the prepared modified steel slag. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.
[0019] Example 1
[0020] (1) First, the steel slag is ground into 30 mesh and sieved. The obtained powder is treated with formic acid in a mixed solvent of ethanol and water in a water bath at a temperature of 50° C. for 1 hour to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0021] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=8), and then adding ammonium dihydrogen phosphate in a ratio of 7:1 by mass of the organic carboxylic acid modified steel slag to ammonium dihydrogen phosphate, heating the mixture in a water bath, wherein the reaction temperature of the water bath is 60° C., and the reaction time of the water bath is 5 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0022] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 30 mesh; the dosage relationship of steel slag powder: organic carboxylic acid: alcohol and water is 2g:20mL:2mL:20mL.
[0023] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.4 mg / L; the Cr(VI) concentration in the solution is 2 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), Cr(VI) concentration: 0.01 mg / L, and detected by atomic emission spectroscopy (ICP-AES), the total chromium Cr concentration: 0.1 mg / L.
[0024] Example 2
[0025] (1) First, the steel slag is ground into 200 mesh and sieved. The obtained powder is treated with acetic acid in a mixed solvent of ethylene glycol and water in a water bath at a temperature of 90° C. for 10 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0026] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=11), and then adding diammonium hydrogen phosphate in a ratio of 7:1 of the mass ratio of the organic carboxylic acid modified steel slag to diammonium hydrogen phosphate, heating the mixture in a water bath, wherein the temperature of the water bath reaction is 90° C., and the reaction time of the water bath is 10 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0027] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 200 mesh; the dosage of steel slag powder: organic carboxylic acid: alcohol and water is 5g:40mL:8mL:40mL.
[0028] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.6 mg / L; the Cr(VI) concentration in the solution is 20 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.09 mg / L, and the total chromium Cr concentration is: 0.7 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0029] Example 3
[0030] (1) First, the steel slag is ground into 60 mesh and sieved. The obtained powder is treated with propionic acid in a mixed solvent of propylene glycol and water in a water bath at a temperature of 70° C. for 5 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0031] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH = 9), and then adding disodium hydrogen phosphate in a ratio of 10:1 by mass of the organic carboxylic acid modified steel slag to disodium hydrogen phosphate, heating the mixture in a water bath, wherein the temperature of the water bath reaction is 70° C., and the reaction time of the water bath reaction is 7 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0032] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 60 mesh; the dosage relationship of steel slag powder: organic carboxylic acid: alcohol and water is 3g:30mL:5mL:30mL.
[0033] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.5 mg / L; the Cr(VI) concentration in the solution is 10 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.05 mg / L, and the total chromium Cr concentration is: 0.6 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0034] Example 4
[0035] (1) First, the steel slag is ground into 100 mesh and sieved. The obtained powder is treated with acetic acid in a mixed solvent of ethanol and water in a water bath at a temperature of 80° C. for 9 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0036] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=10), and then adding dipotassium hydrogen phosphate in a ratio of 8:1 by mass of the organic carboxylic acid modified steel slag to dipotassium hydrogen phosphate, heating the mixture in a water bath, wherein the temperature of the water bath reaction is 80° C., and the reaction time of the water bath reaction is 8 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0037] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 100 mesh; the dosage relationship of steel slag powder: organic carboxylic acid: alcohol and water is 4g:40mL:7mL:30mL.
[0038] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.6 mg / L; the Cr(VI) concentration in the solution is 15 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.07 mg / L, and the total chromium Cr concentration is: 0.7 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0039] Example 5
[0040] (1) First, the steel slag is ground into 150 mesh and sieved. The obtained powder is treated with propionic acid in a mixed solvent of ethanol and water in a water bath at a temperature of 80° C. for 9 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0041] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=10), and then adding sodium dihydrogen phosphate in a ratio of 7.5:1 by mass of the organic carboxylic acid modified steel slag to sodium dihydrogen phosphate, heating the mixture in a water bath for reaction at a temperature of 70° C. for 9 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0042] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 150 mesh; the dosage of steel slag powder: organic carboxylic acid: alcohol and water is 5g:30mL:7mL:40mL.
[0043] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.5 mg / L; the Cr(VI) concentration in the solution is 10 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.06 mg / L, and the total chromium Cr concentration is: 0.6 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0044] Example 6
[0045] (1) First, the steel slag is ground into 180 mesh and sieved. The obtained powder is treated with butyric acid in a mixed solvent of ethanol and water in a water bath at a temperature of 70° C. for 7 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0046] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH = 10), and then adding potassium dihydrogen phosphate in a ratio of 10:1 by mass of the organic carboxylic acid modified steel slag to potassium dihydrogen phosphate, heating the mixture in a water bath, wherein the reaction temperature of the water bath is 80° C., and the reaction time of the water bath is 7 hours, thereby obtaining a carboxyl modified steel slag powder loaded with hydroxyapatite.
[0047] In step (1), steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 180 mesh; the dosage of steel slag powder: organic carboxylic acid: alcohol and water is 5g:40mL:6mL:40mL.
[0048] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.6 mg / L; the Cr(VI) concentration in the solution is 15 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbohydrazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.07 mg / L, and the total chromium Cr concentration is: 0.6 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0049] Example 7
[0050] (1) First, the steel slag is ground into 60 mesh and sieved. The obtained powder is treated with valeric acid in a mixed solvent of ethanol and water in a water bath at a temperature of 80° C. for 8 hours to obtain a carboxyl-modified steel slag powder, in which the carboxyl groups are complexed with Fe ions on the surface.
[0051] (2) dispersing the organic carboxylic acid modified steel slag powder obtained in step (1) in water, adjusting the suspension to be alkaline (pH=10), and then adding diammonium hydrogen phosphate in a ratio of 8.5:1 of the mass ratio of the organic carboxylic acid modified steel slag to diammonium hydrogen phosphate, heating the mixture in a water bath at a temperature of 70° C. for 5 hours to obtain carboxyl modified steel slag powder loaded with hydroxyapatite.
[0052] In step (1), the steel slag is a solid waste material rich in iron and calcium; the particle size of the steel slag powder is 60 mesh; the dosage ratio of the steel slag powder: organic carboxylic acid: alcohol and water is 3g:40mL:5mL:30mL.
[0053] The prepared modified steel slag can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation, wherein preferably, the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.4 mg / L; the Cr(VI) concentration in the solution is 5 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbazide Spectrophotometry" (GB 7467-87), the Cr(VI) concentration is: 0.02 mg / L, and the total chromium Cr concentration is: 0.2 mg / L after atomic emission spectroscopy (ICP-AES) detection.
[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A steel slag conversion method for total chromium removal, It is characterized in that The following steps are involved: (1) First, the steel slag is ground into 30-200 mesh and sieved. The obtained powder is treated with an organic carboxylic acid in a mixed solvent of alcohol and water in a water bath at a temperature of 50-90° C. for 1-10 hours to obtain a carboxyl-modified steel slag powder, wherein the carboxyl group is complexed with Fe ions on the surface; (2) dispersing the powder obtained in step (1) in water, adjusting the suspension to an alkaline pH of 8-11, and then adding phosphate to heat the reaction in a water bath at a temperature of 60-90° C. for 5-10 hours to obtain a carboxyl-modified steel slag powder loaded with hydroxyapatite.
2. The method according to claim 1, It is characterized in that Wherein in step (1), the particle size of the steel slag powder is 60 mesh.
3. The method according to claim 1, It is characterized in that Wherein in step (1), the usage ratio of steel slag powder: organic carboxylic acid: alcohol and water is 2-5g:20-40mL:2-8mL:20-40mL.
4. The method according to claim 1, It is characterized in that Steel slag is a solid waste material rich in iron and calcium; the alcohol is selected from ethanol, ethylene glycol, and glycerol, preferably ethanol.
5. The method according to claim 1, It is characterized in that The organic carboxylic acid is selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, preferably acetic acid.
6. The method according to claim 1, It is characterized in that The phosphate is diammonium hydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, preferably diammonium hydrogen phosphate, and the mass ratio of the organic carboxylic acid modified steel slag to the phosphate is 7-10:1, preferably 9-10:
1.
7. The method according to claim 1, It is characterized in that The suspension was adjusted to pH 8-11 by adding aqueous ammonia.
8. Modified steel slag powder prepared according to the method described in any one of claims 1 to 7.
9. Use of the modified steel slag powder prepared by the method according to any one of claims 1 to 7 can achieve Cr(VI) reduction and adsorption and fixation of Cr(III) products under visible light irradiation.
10. The method according to claim 9 is used to reduce Cr(VI) to Cr(III) under visible light irradiation, and adsorb and fix the obtained Cr(III) product to reduce the total chromium in the solution; the concentration of the modified steel slag powder in the Cr(VI)-containing solution is 0.4-0.6 mg / L; the Cr(VI) concentration in the solution is 2-20 mg / L, preferably 5-15 mg / L; the Cr(VI) concentration in the solution after the reaction is detected by the national standard "Determination of Hexavalent Chromium in Water Quality by Diphenylcarbazide Spectrophotometry" (GB 7467-87), Cr(VI) concentration: ≤0.1 mg / L, and the total chromium Cr concentration is ≤1 mg / L after atomic emission spectroscopy (ICP-AES).
Citation Information
Patent Citations
Steel slag composite adsorbing agent and method for processing printing and dyeing wastewater
CN101716487A
Method for adsorbing and treating chromium-containing wastewater by using steel slag
CN101774671A
Novel Cr (VI) adsorbent and preparation method thereof
CN103182292A
Method for preparing environmental protection material used for sewage treatment by reforming metallurgical dregs
CN105854784A
Adsorbent based on waste steel slag and preparation method and application thereof
CN108554379A