Method for removing silicon in nickel sulfate solution
By using silicon removal adsorbent and filtration pressure treatment in nickel sulfate solution to remove silicon, the complex and unenvironmental problems in the production of nickel sulfate solution are solved, and efficient and stable silicon removal effect is achieved, and removal through high-temperature activation and regeneration is achieved. Silicone slag improves the quality and economic benefits of nickel sulfate products.
Patent Information
- Application Number
- CN202411043074.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art has complicated silicon removal processes and are not environmentally friendly in the production process of nickel sulfate solution, which affects production efficiency and product quality, and silicon pollution has a negative impact on ternary lithium batteries.
The silicon removal adsorbent (such as aluminum oxide, magnesium oxide and lanthanum oxide) is added to the nickel sulfate solution for mixing and removing silicon by filtration. The resulting silicon removal slag can be used through high-temperature activation and regeneration.
The silicon removal effect is achieved with a silicon content dropping from 10 to 40 mg/L to below 5 mg/L. The process is simple and stable, and the temperature and pH range is wide. There is no need for additional thermal energy and pH adjustment. The silicon slag removal can be recycled and recycled. Safety and environmental protection, improving product quality and economic benefits.
Smart Images

Figure CN118957296A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solution impurity removal in a nickel-cobalt hydrometallurgical process, and in particular to a method for removing silicon from a nickel sulfate solution. Background Art
[0002] Nickel sulfate is the main source of nickel for the positive electrode material of ternary lithium batteries. During the mining and smelting of nickel ore, silicon remains in the nickel sulfate solution, affecting production efficiency, product quality, and causing silicon pollution in ternary lithium batteries.
[0003] During the evaporation and crystallization process of nickel sulfate, silicon will precipitate and adhere to the inner wall of the equipment, affecting the evaporation efficiency. Long-term enrichment will cause a large amount of water-insoluble matter in the nickel sulfate product, affecting product quality. Silicon pollution can easily have a negative impact on ternary lithium batteries: (1) Silicon particles will gradually increase with the cycle of the battery, resulting in adhesion failure of the electrode material or electrode separation; (2) The presence of silicon particles will cause fatigue and cracking of the electrode material, reducing the cycle life of the lithium battery; (3) Silicon pollution will reduce the electrochemical reaction of the material and reduce the battery capacity of the lithium battery.
[0004] Purification and silicon removal in the production process of nickel sulfate solution is beneficial to improving production efficiency and product quality. In the prior art, the process of silicon removal in the production process of nickel sulfate solution is complicated; for example, the commonly used resin adsorption silicon removal method requires the use of a large amount of acid, pure water, and alkali solution to desorb, clean and regenerate the resin. The process is complicated and the wastewater output is large, which is not conducive to environmental protection and application. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for removing silicon in a nickel sulfate solution, aiming to solve the problems of complicated process and environmental pollution in the production process of nickel sulfate solution using the existing technology for removing silicon.
[0006] To achieve the above-mentioned purpose, the present invention provides a method for removing silicon from a nickel sulfate solution, comprising adding a silicon removal adsorbent to the nickel sulfate solution, mixing for 30 to 60 minutes to obtain a mixed solution; and performing a filter press treatment on the mixed solution to obtain a silicon-removed liquid and silicon-removed slag.
[0007] Wherein, the dosage of the desiliconizing adsorbent is X, in kg:
[0008] X=C Si ×V×R1×10 -3 ,
[0009] In the formula, C Si is the silicon content in the nickel sulfate solution, in g / m 3 , V is the volume of the nickel sulfate solution, in m 3 , R1 is the reaction coefficient, 800≤R1≤1200.
[0010] The desiliconizing adsorbent includes one or more of aluminum oxide, magnesium oxide and lanthanum oxide.
[0011] Furthermore, the particle size of the desiliconizing adsorbent is 300 meshes.
[0012] Furthermore, the desiliconizing adsorbent is added under the conditions that the temperature of the nickel sulfate solution is 20 to 80° C. and the pH is 3.0 to 6.0.
[0013] Furthermore, the desiliconizing adsorbent is added under the conditions that the temperature of the nickel sulfate solution is 40-60° C. and the pH is 3.0-5.5.
[0014] Furthermore, the desiliconizing adsorbent is alumina.
[0015] Furthermore, the mixing treatment is carried out by mechanically stirring the nickel sulfate solution to which the desiliconizing adsorbent is added; the rotation speed of the mechanical stirring is 60 to 85 r / min.
[0016] Furthermore, the components of the nickel sulfate solution include Ni 90-110 g / L, Si 10-40 mg / L, Co≤2300 mg / L, Ca≤700 mg / L, Mg≤30 mg / L, Mn≤8 mg / L, Pb≤5 mg / L, Cu≤15 mg / L, Zn≤45 mg / L, and Cr≤1 mg / L.
[0017] Furthermore, the filter press treatment method is to use a plate and frame filter press to filter the mixed liquid; wherein, the working pressure per unit area of the plate and frame filter press is 0.10-0.30 MPa; and the pore size of the filter cloth of the plate and frame filter press is 2.0-5.0 μm.
[0018] Furthermore, the method further comprises subjecting the desiliconization slag to high-temperature activation treatment to obtain a regenerated desiliconization adsorbent; wherein the temperature of the high-temperature activation treatment is 500°C.
[0019] Furthermore, the duration of the high temperature activation treatment is 1 hour.
[0020] The beneficial effects achieved by the present invention are:
[0021] The method for removing silicon from nickel sulfate solution provided by the present invention can reduce the silicon content from 10 to 40 mg / L to below 5 mg / L by adding a silicon removal adsorbent to the nickel sulfate solution for mixing treatment, and then performing a filter press treatment; the process operation is simple and the silicon removal effect is stable. The method is applicable to a wide temperature range (20°C to 80°C) without consuming additional heat energy; the method is applicable to a wide pH range (3.0 to 6.0) without adjusting the pH; and other impurities will not be introduced during use.
[0022] Moreover, the silicon removal slag produced in the process of removing silicon from the nickel sulfate solution can be regenerated by high-temperature activation treatment and used again to remove silicon from the nickel sulfate solution. The number of regeneration cycles can reach more than 20 times. The method for removing silicon from the nickel sulfate solution also has the advantages of no waste water and waste gas generation, and the use process is safe and environmentally friendly. The method for removing silicon from the nickel sulfate solution can effectively improve the quality of nickel sulfate products, has high economic benefits and practical value, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0024] Figure 1 The present invention is a schematic flow chart of a method for removing silicon from a nickel sulfate solution according to an optional embodiment of the present invention.
[0025] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments rather than to limit the scope of protection of the present invention.
[0028] Unless otherwise defined, all technical and scientific terms used in the present invention are consistent with the prior art knowledge of those skilled in the art and the description of the present invention. The present invention can also be implemented using any methods, devices and materials in the prior art that are similar or equivalent to the methods, devices and materials described in the embodiments of the present invention.
[0029] When the embodiments give numerical ranges, it should be understood that unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. The test methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers. The materials or reagents required in the following embodiments are commercially available unless otherwise specified.
[0030] In order to solve the problems of complicated process and environmental pollution in removing silicon in the production process of nickel sulfate solution using the existing technology, the present invention provides a method for removing silicon in nickel sulfate solution, comprising adding a silicon removal adsorbent to the nickel sulfate solution, mixing for 30 to 60 minutes to obtain a mixed solution; and performing filter press treatment on the mixed solution to obtain a silicon-removed liquid and silicon-removed slag.
[0031] Among them, the amount of silicon removal adsorbent is X, in kg:
[0032] X=C Si ×V×R1×10 -3 ,
[0033] In the formula, C Si is the silicon content in nickel sulfate solution, in g / m 3 , V is the volume of nickel sulfate solution, unit is m 3 , R1 is the reaction coefficient, 800≤R1≤1200. Specifically, the mass of the silicon removal adsorbent added to the nickel sulfate solution is 800 to 1200 times the total mass of silicon in the nickel sulfate solution, for example, it can be 800 times, 900 times, 1000 times, 1100 times or 1200 times. In an optional embodiment, the flow diagram of the method for removing silicon from the nickel sulfate solution is as follows Figure 1 shown.
[0034] The desiliconizing adsorbent includes one or more of aluminum oxide, magnesium oxide and lanthanum oxide. Specifically, the desiliconizing adsorbent (one or more of aluminum oxide, magnesium oxide and lanthanum oxide) is positively charged, and the silicon-containing groups in the nickel sulfate solution are negatively charged. Charge adsorption occurs in the system, and the silicon-containing groups in the nickel sulfate solution have a good adsorption effect. After the reaction, solid-liquid separation is performed by filter pressing to achieve desiliconization.
[0035] The method for removing silicon from nickel sulfate solution provided by the present invention can reduce the silicon content from 10 to 40 mg / L to below 5 mg / L by adding a silicon removal adsorbent to the nickel sulfate solution for mixing treatment, and then performing a filter press treatment; the process operation is simple and the silicon removal effect is stable. The method is applicable to a wide temperature range (20°C to 80°C) without consuming additional heat energy; the method is applicable to a wide pH range (3.0 to 6.0) without adjusting the pH; and other impurities will not be introduced during use.
[0036] Moreover, the silicon removal slag produced in the process of removing silicon from the nickel sulfate solution can be regenerated by high-temperature activation treatment and used again to remove silicon from the nickel sulfate solution. The number of regeneration cycles can reach more than 20 times. The method for removing silicon from the nickel sulfate solution also has the advantages of no waste water and waste gas generation, and the use process is safe and environmentally friendly. The method for removing silicon from the nickel sulfate solution can effectively improve the quality of nickel sulfate products, has high economic benefits and practical value, and has broad application prospects.
[0037] Furthermore, the particle size of the desiliconizing adsorbent is 300 mesh. Specifically, the particle sizes of the aluminum oxide, magnesium oxide and lanthanum oxide used are all 300 mesh. If the particle size of the desiliconizing adsorbent is small, it is easy to dissolve and contaminate the nickel sulfate solution; if the particle size of the desiliconizing adsorbent is large, its specific surface area is small, the amount of desiliconizing adsorbent required is larger, and the adsorption efficiency is lower. In summary, it is appropriate to use a desiliconizing adsorbent with a particle size of 300 mesh.
[0038] Furthermore, a desiliconizing adsorbent is added to the nickel sulfate solution at a temperature of 20 to 80° C. and a pH of 3.0 to 6.0.
[0039] Furthermore, a desiliconizing adsorbent is added to the nickel sulfate solution at a temperature of 40 to 60° C. and a pH of 3.0 to 5.5.
[0040] Furthermore, the silicon removal adsorbent is alumina.
[0041] Furthermore, the mixing treatment is carried out by mechanically stirring the nickel sulfate solution to which the desiliconizing adsorbent is added; the speed of the mechanical stirring is 60 to 85 r / min. Specifically, the nickel sulfate solution to which the desiliconizing adsorbent is added is mechanically stirred using a stirred reactor; the speed of the stirred reactor can be 60 r / min, 65 r / min, 70 r / min, 75 r / min, 80 r / min or 85 r / min.
[0042] Furthermore, the components of the nickel sulfate solution include Ni 90-110 g / L, Si 10-40 mg / L, Co≤2300 mg / L, Ca≤700 mg / L, Mg≤30 mg / L, Mn≤8 mg / L, Pb≤5 mg / L, Cu≤15 mg / L, Zn≤45 mg / L, and Cr≤1 mg / L. Specifically, the nickel sulfate solution is a silicon removal pre-liquid obtained after most of the impurity iron is removed by adding alkali, heating, and adding an oxidant for precipitation in a conventional nickel sulfate impurity removal process. The temperature of the silicon removal pre-liquid (nickel sulfate solution) obtained by the impurity removal process is between 40°C and 60°C, and the pH is between 3.0 and 5.5; and the components of the nickel sulfate solution include Ni 90-110g / L, Si 10-40mg / L, Co≤2300mg / L, Ca≤700mg / L, Mg≤30mg / L, Mn≤8mg / L, Pb≤5mg / L, Cu≤15mg / L, Zn≤45mg / L, and Cr≤1mg / L.
[0043] Furthermore, the filter press treatment method is to use a plate and frame filter press to filter the mixed liquid; wherein the working pressure per unit area of the plate and frame filter press is 0.10-0.30 MPa; the filter cloth pore size of the plate and frame filter press is 2.0-5.0 μm. Specifically, the working pressure per unit area of the plate and frame filter press can be 0.10 MPa, 0.15 MPa, 0.20 MPa, 0.25 MPa or 0.30 MPa; preferably 0.25 MPa. The filter cloth pore size of the plate and frame filter press can be 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm, 5.0 μm; preferably 2.0 μm.
[0044] Furthermore, the method further comprises subjecting the desiliconizing slag to high temperature activation treatment to obtain a regenerated desiliconizing adsorbent, wherein the temperature of the high temperature activation treatment is 500° C. Specifically, when the temperature of the high temperature activation treatment is low, the activation effect cannot be achieved; and when the temperature is too high, the desiliconizing adsorbent will agglomerate and increase energy consumption.
[0045] Furthermore, the duration of the high temperature activation treatment is 1 hour. Specifically, if the duration of the high temperature activation treatment is too short, the Guohua effect will not be achieved; if the duration is too long, unnecessary energy consumption will be increased.
[0046] For further understanding of the present invention, examples are given below:
[0047] Example 1
[0048] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 24.0m 3 , Nickel: 105.1g / L, Silicon: 27.3mg / L.
[0049] (1) Detection: The temperature of the nickel sulfate solution was 48.4°C, pH was 5.2, and silicon was 27.3 mg / L. The temperature and pH of the nickel sulfate solution were within the applicable range of the silicon removal adsorbent, and alumina (silicon removal adsorbent) with a particle size of 300 mesh could be directly added.
[0050] (2) Calculation: According to the formula "X = C Si ×V×R1×10 -3 ", taking R1 = 1000, calculate the amount of silicon removal adsorbent (X) = 27.3 × 24.0 × 1000 × 10 -3 =655.2kg, take 660kg.
[0051] (3) Silicon removal: at 24.0m 3 660 kg of desiliconizing adsorbent was added to the nickel sulfate solution, stirred at a speed of 80 r / min, and reacted for 60 min.
[0052] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 3.6 mg / L, which met the requirements.
[0053] Example 2
[0054] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 30.0m 3 , Nickel: 107.4g / L, Silicon: 32.6mg / L.
[0055] (1) Detection: The temperature of the nickel sulfate solution was 51.3°C, pH was 5.4, and silicon was 32.6 mg / L. The temperature and pH of the nickel sulfate solution were within the applicable range of the silicon removal adsorbent, and alumina (silicon removal adsorbent) with a particle size of 300 mesh could be directly added.
[0056] (2) Calculation: According to the formula "X = C Si ×V×R1×10 -3 ", take R1 = 900, calculate the amount of silicon removal adsorbent (X) = 32.6 × 30.0 × 900 × 10 -3 =880.2kg, take 880kg.
[0057] (3) Silicon removal: at 30.0m 3 880 kg of desiliconizing adsorbent was added to the nickel sulfate solution, stirred at a speed of 75 r / min, and reacted for 50 minutes.
[0058] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 4.1 mg / L, which met the requirements.
[0059] Example 3
[0060] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 25.0m 3 , Nickel: 104.9g / L, Silicon: 18.5mg / L.
[0061] (1) Detection: The temperature of the nickel sulfate solution was 49.7°C, pH was 5.1, and silicon was 18.5 mg / L. The temperature and pH of the nickel sulfate solution were within the applicable range of the silicon removal adsorbent, and lanthanum oxide (silicon removal adsorbent) with a particle size of 300 mesh could be directly added.
[0062] (2) Calculation: According to the formula "X = C Si ×V×R1×10 -3 ", take R1 = 1100, calculate the amount of silicon removal adsorbent (X) = 18.5 × 25.0 × 1100 × 10 -3 =508.8kg, take 510kg.
[0063] (3) Silicon removal: at 25.0m 3 510 kg of desiliconizing adsorbent was added to the nickel sulfate solution, stirred at a speed of 75 r / min, and reacted for 60 minutes.
[0064] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 2.8 mg / L, which met the requirements.
[0065] Example 4
[0066] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 30.0m 3 , nickel: 100.2g / L, silicon: 22.8mg / L.
[0067] (1) Detection: The temperature of the nickel sulfate solution is 45.0°C, the pH is 4.8, and the silicon is 22.8 mg / L. If the temperature and pH of the nickel sulfate solution are within the applicable range of the silicon removal adsorbent, the silicon removal adsorbent can be directly added.
[0068] (2) Calculation: According to the formula "X = C Si ×V×R1×10 -3 ", take R1 = 1200, calculate the amount of silicon removal adsorbent = 22.8 × 30.0 × 1200 × 10 -3 (kg) = 820.8kg, take 820kg of the desiliconization slag produced in Example 2 after activation (regenerated desiliconization adsorbent).
[0069] (3) Silicon removal: at 30.0m3 820 kg of regenerated desiliconizing adsorbent was added to the nickel sulfate solution, stirred at a speed of 70 r / min, and reacted for 40 minutes.
[0070] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 2.3 mg / L, which met the requirements.
[0071] Comparative Example 1
[0072] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 24.0m 3 , Nickel: 105.1g / L, Silicon: 27.3mg / L.
[0073] (1) Detection: The temperature of the nickel sulfate solution was 48.4°C, pH was 5.2, and silicon was 27.3 mg / L. The temperature and pH of the nickel sulfate solution were within the applicable range of the silicon removal adsorbent, and alumina (silicon removal adsorbent) with a particle size of 300 mesh could be directly added.
[0074] (2) Calculation: According to the formula "X = C Si ×V×R1×10 -3 ", taking R1 = 1000, calculate the amount of silicon removal adsorbent (X) = 27.3 × 24.0 × 1000 × 10 -3 =655.2kg, take 660kg.
[0075] (3) Silicon removal: at 24.0m 3 Add 660 kg of desiliconizing adsorbent to the nickel sulfate solution, stir at a speed of 80 r / min, and react for 15 minutes.
[0076] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 8.4 mg / L, which did not meet the requirements.
[0077] Comparative Example 2
[0078] Nickel sulfate solution (pre-silicon removal solution after iron removal), volume: 24.0m 3 , Nickel: 105.1g / L, Silicon: 27.3mg / L.
[0079] (1) Detection: The temperature of the nickel sulfate solution was 48.4°C, pH was 5.2, and silicon was 27.3 mg / L. The temperature and pH of the nickel sulfate solution were within the applicable range of the silicon removal adsorbent, and alumina (silicon removal adsorbent) with a particle size of 300 mesh could be directly added.
[0080] (2) Calculation: According to the formula "X = CSi ×V×R1×10 -3 ", take R1 = 600, calculate the amount of silicon removal adsorbent (X) = 27.3 × 24.0 × 600 × 10 -3 =393.1kg, take 390kg.
[0081] (3) Silicon removal: at 24.0m 3 390 kg of desiliconizing adsorbent was added to the nickel sulfate solution, stirred at a speed of 80 r / min, and reacted for 60 min.
[0082] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25 MPa and the pore size of the filter cloth was 2.0 μm. The desiliconized liquid and desiliconized slag were obtained by filtration. The silicon content of the desiliconized liquid was 11.5 mg / L, which did not meet the requirements.
[0083] In summary, the above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for removing silicon from a nickel sulfate solution, characterized in that: The method comprises adding a desiliconizing adsorbent to a nickel sulfate solution, mixing the solution for 30 to 60 minutes, and obtaining a mixed solution; Performing filter pressing treatment on the mixed liquid to obtain desiliconized liquid and desiliconized slag; Wherein, the dosage of the desiliconizing adsorbent is X, in kg: X=C Si ×V×R1×10 -3 , In the formula, C Si is the silicon content in the nickel sulfate solution, in g / m 3 , V is the volume of the nickel sulfate solution, in m 3 , R1 is the reaction coefficient, 800≤R1≤1200; The desiliconizing adsorbent includes one or more of aluminum oxide, magnesium oxide and lanthanum oxide.
2. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The particle size of the desiliconizing adsorbent is 300 meshes.
3. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The desiliconizing adsorbent is added under the conditions that the temperature of the nickel sulfate solution is 20 to 80° C. and the pH value is 3.0 to 6.
0.
4. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The desiliconizing adsorbent is added under the conditions that the temperature of the nickel sulfate solution is 40-60° C. and the pH value is 3.0-5.
5.
5. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The desiliconizing adsorbent is alumina.
6. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The mixing treatment method is to mechanically stir the nickel sulfate solution to which the desiliconizing adsorbent is added; the rotation speed of the mechanical stirring is 60 to 85 r / min.
7. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The components of the nickel sulfate solution include Ni 90-110 g / L, Si 10-40 mg / L, Co≤2300 mg / L, Ca≤700 mg / L, Mg≤30 mg / L, Mn≤8 mg / L, Pb≤5 mg / L, Cu≤15 mg / L, Zn≤45 mg / L, and Cr≤1 mg / L.
8. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The filter press treatment method is to use a plate and frame filter press to filter the mixed liquid; Wherein, the working pressure per unit area of the plate and frame filter press is 0.10-0.30 MPa; and the pore size of the filter cloth of the plate and frame filter press is 2.0-5.0 μm.
9. The method for removing silicon from a nickel sulfate solution according to claim 1, characterized in that: The invention also includes subjecting the desiliconization slag to high temperature activation treatment to obtain a regenerated desiliconization adsorbent; Wherein, the temperature of the high temperature activation treatment is 500°C.
10. The method for removing silicon from a nickel sulfate solution according to claim 9, characterized in that: The duration of the high temperature activation treatment is 1 hour.