Method for smelting tin-containing material by intermittently spraying vulcanizing agent in molten pool
Through the intermittent melt pool spraying method, the problems of low vulcanization efficiency and high energy consumption in the vulcanization treatment of tin-containing materials are solved, the utilization rate of vulcanizing agent and tin recovery efficiency are improved, energy consumption and furnace body corrosion are reduced, and the utilization rate of vulcanizing agent is reduced. Higher economic benefits.
Patent Information
- Application Number
- CN202411025010.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the vulcanization efficiency and high energy consumption during the vulcanization treatment of tin-containing materials lead to a decrease in tin recovery rate and furnace body corrosion, which affects economic benefits.
The method of spraying vulcanizing agent in batch type melt pool is used to spray the dried vulcanizing agent intermittently through the second spray gun, combining the injection of pulverized coal and air, promote the vulcanization reaction, and improve the utilization rate and reaction rate of vulcanizing agent. , reduce the heat load of the smoke furnace.
The utilization rate of vulcanizing agent is increased by 30-50%, energy consumption and carbon consumption are reduced, furnace body life is extended, tin recycling cost is reduced by 20-30%, and smelting efficiency is improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool. Background Art
[0002] Tin is an important metal raw material supporting the development of the national economy. With the progress of society and the development of mankind, tin has gradually become an indispensable key rare metal in modern industry. It is mainly used in the production of tinplate, electroplating, corrosion science, welding, materials, tin chemical products and other metallurgical uses of tin. It is widely used in electronics, information, electrical appliances, chemicals, metallurgy, building materials, machinery, food packaging, aerospace, ships, fuel, atomic energy and spacecraft and other cutting-edge technology fields. It is called "industrial MSG".
[0003] For a long time, the fuming furnace sulfidation volatilization method has been mainly used to treat tin-containing materials. The fuming furnace sulfidation volatilization method takes advantage of the high vapor pressure of stannous sulfide. The sulfiding agent is added to the fuming furnace from the fuming furnace feed port. Under the intense stirring of pulverized coal and air sprayed by the spray gun, tin volatilizes in the form of tin sulfide and oxidizes in the upper part of the fuming furnace, and is finally recovered in the form of stannous oxide smoke.
[0004] Chinese patent application ZL200810233554.0 discloses a method for oxygen-enriched smelting of low-tin materials in a fuming furnace. The method adopts oxygen-enriched smelting in the process of smelting low-tin materials in a fuming furnace, mixes oxygen into the secondary air, and increases the amount of oxygen added to the molten pool per unit time under the condition that the total air volume put into the furnace per unit time remains unchanged, and the amount of fuel, energy and material processed put into the furnace per unit time increases synchronously, and the output of tin smoke also increases accordingly. This process method further improves the smelting speed and efficiency, reduces the amount of smoke per unit material, increases the output of tin smoke, and improves the tin content of the smoke.
[0005] Chinese patent application ZL200710066225.7 discloses a new process for recovering tin by volatilization in a fuming furnace. A waste heat boiler is set on the flue system of the fuming furnace to recover heat, and a dry bag dust collector is used in the subsequent dust collection device. The total recovery rate of tin in this process is high, and the heat in the recovery can be fully released and utilized, which greatly reduces the temperature of the subsequent dry dust collection, and does not generate industrial wastewater.
[0006] Chinese patent application ZL202010928573.6 discloses a smelting furnace and smelting method for continuous fuming of low-grade tin materials. The smelting furnace includes a smelting furnace, a fuming furnace, and a water-cooled slag channel; the smelting furnace is a side-blown oxygen-enriched smelting furnace, including a square furnace body, a smelting furnace charging port and a smelting furnace flue gas outlet arranged at the top of the furnace body, a smelting furnace nozzle arranged on the front and rear sides of the furnace body, an oxygen-enriched air duct and a smelting furnace fuel pipe; the fuming furnace is a side-blown sulfurization volatilization furnace, including a square furnace body, a sulfiding agent inlet and a fuming furnace flue gas outlet arranged at the top of the furnace body, a fuming furnace nozzle arranged on the front and rear sides of the furnace body, a fuming furnace fuel pipe and an air input pipe, and a slag outlet arranged on one side of the fuming furnace. This technical solution can complete the two metallurgical processes of continuous melting and continuous sulfidation of low-grade tin materials in one step, with a short operation process, low cost, high tin recovery rate, and good energy-saving effect.
[0007] However, the addition of the sulfiding agent in the above patents is directly added from the feeding port of the fuming furnace, which has the following problems: (1) The sulfiding agent used in industry is obtained after ore dressing, and the sulfiding agent contains more than 30% water. After entering the furnace, it absorbs a large amount of heat, which increases the heat load of the fuming furnace. At the same time, a large amount of water is generated, which causes corrosion to the fuming furnace and affects the life of the fuming furnace; (2) The sulfiding agent can only be added to the local surface of the molten pool, and the contact area with the molten pool is small, the reaction rate is slow, and the sulfidation efficiency is low; (3) The sulfiding agent cannot be completely dispersed in the molten pool, which is easy to cause local excess and generate tin matte. Tin matte will reduce the vapor pressure of stannous sulfide and dissolve part of tin, thereby reducing the recovery rate of tin. In order to solve this problem in industry, the air injection amount is usually increased to make the local excess sulfiding agent oxidize and form slag. Excessive air injection increases the flue gas volume and takes away a lot of heat. In order to maintain the thermal balance in the furnace, more pulverized coal must be injected at the same time, thereby increasing energy consumption and carbon consumption, affecting economic benefits. Summary of the invention
[0008] The main purpose of the present invention is to provide a method for smelting tin-containing materials by spraying a sulfiding agent in an intermittent molten pool, so as to solve the problems of low sulfidation efficiency and high energy consumption in the sulfidation treatment process of tin-containing materials in the prior art.
[0009] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for smelting tin-containing materials by spraying a sulfiding agent in an intermittent molten pool is provided, which comprises: a feeding process: adding a mixture of the tin-containing material and the flux into the fuming furnace from the feeding port of the fuming furnace, and spraying a mixture of pulverized coal and air into the fuming furnace through a first spray gun, so that the tin-containing material is melted to form a molten pool during the heat release of the pulverized coal combustion; during the melting of the tin-containing material, intermittently spraying a dried sulfiding agent into the molten pool through a second spray gun; a sulfidation reaction process: stopping the feeding of the mixture, and continuing to spray the mixture of pulverized coal and air, and at the same time continuing to intermittently spray the dried sulfiding agent into the molten pool, so that the tin undergoes a sulfidation reaction under stirring, volatilizes in the form of stannous sulfide, and is oxidized in the flue gas flow at the upper part of the fuming furnace to form stannous oxide and discharged from the fuming furnace.
[0010] Furthermore, during the feeding process, the mixed material is added in batches; when more than half of the total amount of the mixed material added to the furnace is added, the dried vulcanizing agent is intermittently sprayed into the molten pool through the second spray gun.
[0011] Furthermore, during the feeding process, the mixture is added in the form of 5 to 20 batches, and the feeding time for each batch is 5 to 20 minutes; when more than half of the total amount of the mixture has been added to the furnace, the dried vulcanizing agent is intermittently sprayed into the molten pool 2 to 3 times through the second spray gun, and each spraying lasts 3 to 5 minutes.
[0012] Furthermore, during the vulcanization reaction, the dried vulcanizing agent is intermittently sprayed into the molten pool 2 to 5 times, and each spraying lasts for 5 to 10 minutes.
[0013] Furthermore, the total duration of the feeding process is 0.5 to 1.5 hours, and the total duration of the vulcanization reaction process is 1 to 2 hours.
[0014] Furthermore, the second spray gun is a single-channel spray gun, and the diameter of the spray gun air outlet is 15-25 mm; when the second spray gun sprays the dried vulcanizing agent, nitrogen or air is used as the carrier gas, the spraying pressure is 0.1-0.15 MPa, and the loading amount of the vulcanizing agent is 5-30 kg / Nm 3 The first spray gun is a single-channel spray gun, and the diameter of the spray gun air port is 15-25mm; when the first spray gun sprays the mixture of pulverized coal and air, the spray pressure is 0.1-0.15Mpa, and the load of pulverized coal is 5-30kg / Nm 3 .
[0015] Furthermore, there are multiple second spray guns, and the multiple second spray guns are evenly spaced and arranged on the side of the fuming furnace and in the horizontal direction of the fuming furnace; a first spray gun is arranged between two adjacent second spray guns.
[0016] Furthermore, the height between the first spray gun and the second spray gun and the bottom wall of the fuming furnace is h, and the total height of the furnace body inside the fuming furnace is H, then h / H=1 / 15~1 / 5.
[0017] Furthermore, the vulcanizing agent is pyrite and / or pyrrhotite; preferably, the particle size of the vulcanizing agent is 38-74 μm; preferably, the water content of the dried vulcanizing agent is less than 1%.
[0018] Furthermore, the flux is one or more of siliceous flux, calcic flux and ferrous flux; preferably, the siliceous flux is one or more of quartz, silica and quartz sand; preferably, the calcic flux is one or more of quicklime, slaked lime and limestone; preferably, the ferrous flux is one or more of iron ore and fumed slag.
[0019] The present invention strengthens the vulcanization process of the tin-containing material by changing the addition method of the vulcanizing agent, improves the vulcanization efficiency of the vulcanizing agent, and reduces the amount of the vulcanizing agent used. At the same time, the present invention reduces the energy consumption and carbon consumption of the vulcanization volatilization process in the fuming furnace, also reduces the processing cost of tin recovery, and improves the economic benefits of tin smelting. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0021] As described in the background technology section, the prior art has the problems of low sulfurization efficiency and high energy consumption in the sulfurization treatment process of tin-containing materials. In order to solve this problem, the present invention provides a method for smelting tin-containing materials by spraying a sulfurizing agent in an intermittent molten pool, comprising:
[0022] Feeding process: a mixture of tin-containing material and flux is added into the fuming furnace through the feeding port of the fuming furnace, and a mixture of pulverized coal and air is sprayed into the fuming furnace through the first spray gun, and the tin-containing material is melted to form a molten pool during the heat release of the pulverized coal combustion; during the melting of the tin-containing material, the dried vulcanizing agent is intermittently sprayed into the molten pool through the second spray gun;
[0023] Sulfidation reaction process: stop adding the mixed material, and continue to spray the mixture of pulverized coal and air, and continue to intermittently spray the dried sulfiding agent into the molten pool, so that the tin undergoes a sulfidation reaction under stirring, volatilizes in the form of stannous sulfide, and oxidizes in the flue gas flow at the top of the fuming furnace to form stannous oxide and discharges from the fuming furnace.
[0024] The above method is used to treat tin-containing materials. First, the tin-containing materials are added to the fuming furnace from the fuming furnace feeding port. The tin-containing materials are melted in the heat release process of the pulverized coal combustion by using the pulverized coal and air sprayed by the first spray gun. At the same time, the dried sulfiding agent is intermittently sprayed into the molten pool by the second spray gun. With the intense stirring of the molten pool by the sprayed sulfiding agent, the tin volatilizes in the form of stannous sulfide and is oxidized in the flue gas flow at the top of the fuming furnace, and finally recovered in the form of stannous oxide smoke.
[0025] In the method provided by the present invention, the second spray gun sprays the dried sulfiding agent, which can reduce the consumption of coal in the smelting process and reduce the cost of subsequent water treatment. The smelting of tin-containing materials is carried out by spraying the sulfiding agent in an intermittent molten pool, especially the intermittent sulfiding agent spraying method runs through the entire feeding process and the sulfidation reaction process, effectively reducing the heat load of the fuming furnace, improving the smelting efficiency of tin-containing materials, reducing furnace corrosion, and increasing the life of the furnace. At the same time, the above-mentioned sulfiding agent Oenru method promotes the uniform distribution of the sulfiding agent in the molten pool, fully contacts the materials in the molten pool in all stages, has a fast reaction rate, high sulfidation efficiency, and the utilization rate of the sulfiding agent is effectively increased. Therefore, the present invention can effectively reduce the amount of sulfiding agent added in the smelting process of tin-containing materials, reduce the energy consumption and carbon consumption per ton of slag in the fuming furnace, reduce the content of SO2 in the flue gas, and thus reduce the treatment cost of sulfur dioxide.
[0026] In summary, the present invention effectively solves the problems of low vulcanization efficiency and high energy consumption in the prior art in the vulcanization treatment process of tin-containing materials, can increase the utilization rate of the vulcanizing agent by 30-50%, and comprehensively reduce the recycling cost of low-tin materials by 20-30%, with very considerable economic benefits. Especially in the current boom of recycled metal recycling, the use of this method to recycle low-tin materials is of great significance.
[0027] In order to make the feeding process, melting process and vulcanization process more stable, in a preferred embodiment, during the feeding process, the mixed material is added in the form of batch feeding; when more than half of the total amount of the mixed material added to the furnace is added, the dried vulcanizing agent is sprayed into the molten pool intermittently through the second spray gun. The feeding rhythm is controlled in the above manner, and the intermittently sprayed vulcanizing agent can better contact with the material, thereby further improving the vulcanization efficiency and increasing the utilization rate of the vulcanizing agent.
[0028] More preferably, during the above-mentioned feeding process, the mixture is added in the form of 5 to 20 batches, and the feeding time for each batch is 5 to 20 minutes; when more than half of the total amount of the mixture is added to the furnace, the dried vulcanizing agent is intermittently sprayed into the molten pool 2 to 3 times through the second spray gun, and each spray lasts 3 to 5 minutes. The intermittent spraying of the vulcanizing agent during the feeding period in the above manner can promote a more thorough mixing of the vulcanizing agent with the system during the melting stage, so as to achieve higher reaction efficiency, higher utilization rate of the vulcanizing agent, and lower carbon consumption of the fuming furnace. In order to further improve the efficiency of the vulcanization reaction and increase the utilization rate of the vulcanizing agent during the vulcanization reaction, in a preferred embodiment, during the above-mentioned vulcanization reaction, the dried vulcanizing agent is intermittently sprayed into the molten pool 2 to 5 times, and each spray lasts 5 to 10 minutes.
[0029] The materials in the feeding stage are fully melted, which is fully prepared for the vulcanization reaction in the subsequent vulcanization stage, thereby improving the reaction environment in the entire molten pool, having better stability and uniformity, and better reaction effect. In a preferred embodiment, the total duration of the above-mentioned feeding process is 0.5 to 1.5 hours, and the total duration of the vulcanization reaction process is 1 to 2 hours.
[0030] In addition to the intermittent spraying method that can promote the efficient use of the vulcanizing agent during the feeding and vulcanization process, the unknown method and spraying amount of the spray gun also affect the full contact of the vulcanizing agent to a certain extent. For this purpose, further modification is made. In a preferred embodiment, the second spray gun is a single-channel spray gun, and the diameter of the spray gun air outlet is 15-25 mm; when the second spray gun sprays the dried vulcanizing agent, nitrogen or air is used as the carrier gas, the spraying pressure is 0.1-0.15 MPa, and the loading amount of the vulcanizing agent is 5-30 kg / Nm 3 The first spray gun is a single-channel spray gun with a spray gun tuyere diameter of 15-25 mm. When the first spray gun sprays a mixture of pulverized coal and air, the spray pressure is 0.1-0.15 MPa and the pulverized coal load is 5-30 kg / Nm 3 More preferably, there are multiple second spray guns, and the multiple second spray guns are evenly spaced and arranged at the side of the fuming furnace and horizontally arranged along the fuming furnace; and a first spray gun is arranged between two adjacent second spray guns.
[0031] In the height direction, in order to make the material spraying more uniform, in a preferred embodiment, the height between the first spray gun and the second spray gun and the bottom wall of the fuming furnace is h, and the total height of the furnace body inside the fuming furnace is H, then h / H=1 / 15~1 / 5.
[0032] The above-mentioned vulcanizing agent can be a common type in the art, such as but not limited to pyrite and / or pyrrhotite. In order to make the vulcanizing agent more evenly distributed and thus better promote the efficient vulcanization reaction, preferably, the particle size of the vulcanizing agent is 38-74 μm; more preferably, the water content of the dried vulcanizing agent is less than 1%. For cost considerations, it is preferred to control the water content of the dried vulcanizing agent to be 0.2-1%.
[0033] In a preferred embodiment, the flux is one or more of siliceous flux, calcic flux and ferrous flux; preferably, the siliceous flux is one or more of quartz, silica and quartz sand; preferably, the calcic flux is one or more of quicklime, slaked lime and limestone; preferably, the ferrous flux is one or more of iron ore and fumed slag.
[0034] The above method is used for a variety of tin-containing materials, such as low-sulfur tin middlings (by weight percentage, containing 2% to 10% Sn, 1% to 5% S, 35% to 50% Fe, 1% to 5% SiO2, and 1% to 5% CaO), tin secondary concentrates (by weight percentage, containing 5% to 10% Sn, 2% to 5%, 35% to 50% S, 1% to 5% Fe, and 1% to 5% SiO2), and liquid low-tin reducing slag (by weight percentage, containing 3% to 10% Sn, 0.1% to 3% S, 30% to 40% Fe, 15% to 25% SiO2, and 2% to 5% CaO), etc., which can be one of them or a mixture of several tin-containing materials. In actual operation, low-sulfur tin middlings, tin secondary concentrates, and high-sulfur tin middlings can be directly added to the fuming furnace through the charging port, and liquid low-tin reducing slag can be fed into the fuming furnace charging port through the slag chute for feeding.
[0035] In summary, the method provided by the present invention is used to smelt tin-containing materials, which has the advantages of high efficiency, high utilization rate of the vulcanizing agent, and low energy consumption. The tin content in the slag is less than 0.15%, the utilization rate of the vulcanizing agent is increased by 30% to 50%, the energy consumption is reduced by 15% to 20%, and the content of SO2 in the flue gas is reduced by 15% to 30%.
[0036] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0037] Comparative Example 1
[0038] This comparative example provides a test in which a conventional vulcanizing agent is directly added from a feed port to a fuming furnace to perform smelting of tin-containing materials:
[0039] Low-sulfur tin middlings (containing Sn 3.1%, S2.5%, Fe 38.2%, SiO2 2.3%, CaO 1.6%), tin secondary concentrates (containing Sn 5.2%, S 3.3%, Fe 37.1%, SiO2 3.1%, CaO 2.1%) and flux (SiO2) are mixed and added into the fuming furnace at one time through the feeding port of the fuming furnace, and liquid low-tin reducing slag (containing Sn 3.3%, S2.6%, Fe 35.1%, SiO2 20.3%, CaO 3.5%) flows into the fuming furnace through the slag flow channel and the slag inlet of the fuming furnace, and the mass ratio of low-sulfur tin middlings, tin secondary concentrates, liquid low-tin reducing slag and flux is 3:3:3:1. The oxygen-coal spray gun sprays a mixture of pulverized coal and air to melt the material. After 1.0h of feeding, pyrite containing about 30wt% of water is directly added into the fuming furnace from the feeding port of the fuming furnace. The tin volatilizes in the form of stannous sulfide and is oxidized in the flue gas flow at the top of the fuming furnace and is finally recovered in the form of stannous oxide dust.
[0040] Example 1
[0041] Low-sulfur tin middlings (containing 3.1% Sn, 2.5% S, 38.2% Fe, 2.3% SiO2 and 1.6% CaO), secondary tin concentrates (containing 5.2% Sn, 3.3% S, 37.1% Fe, 3.1% SiO2 and 2.1% CaO) and flux (SiO2) are mixed and added into the fuming furnace through the feeding port. Liquid low-tin reducing slag (containing 3.3% Sn, 2.6% S, 35.1% Fe, 20.3% SiO2 and 3.5% CaO) flows into the fuming furnace through the slag flow channel and the slag inlet of the fuming furnace in 10 batches. The mass ratio of low-sulfur tin middlings, secondary tin concentrates, liquid low-tin reducing slag and flux is 3:3:3:1. The oxygen-coal spray gun sprays a mixture of pulverized coal and air to melt the material. After adding 5 batches of materials, the dried pyrite is sprayed into the molten pool intermittently by the spray gun. It is sprayed twice during the melting period, each time for 3 minutes. After stopping the feeding, it enters the sulfidation period. The oxygen-coal spray gun is a single-channel spray gun with a spray gun tuyere diameter of 20mm. It uses air transportation with a pressure of 0.15Mpa and a coal powder load of 10kg / Nm 3 During the sulfidation period, the sulfiding agent is sprayed intermittently 3 times with a spray gun, each spraying for 5 minutes. The moisture content of the pyrite after drying is 1%, and the particle size below 74μm accounts for 90%. The diameter of the sulfiding agent spray gun is 25mm, and air transportation is adopted with a pressure of 0.15Mpa. Under intense stirring, the tin volatilizes in the form of stannous sulfide and is oxidized in the flue gas flow at the top of the fuming furnace, and finally recovered in the form of stannous oxide smoke. There are 6 sulfiding agent spray guns, which are arranged at equal intervals on the side of the fuming furnace and arranged in the horizontal direction of the fuming furnace; an oxygen-coal spray gun is arranged between two adjacent sulfiding agent spray guns, and the spray gun is arranged at a position where h / H is 2 / 15.
[0042] Example 2
[0043] The difference from Example 1 is that when the vulcanizing agent is sprayed, it is sprayed 3 times during the melting period, each time for 4 minutes, and after stopping the feeding, it enters the vulcanization period. During the vulcanization period, the vulcanizing agent is sprayed intermittently 4 times by a spray gun, each time for 7 minutes. The pyrite contains 0.5% water after drying, and the particle size is below 48μm, accounting for 90%, the diameter of the spray gun tuyere is 20mm, and the air delivery pressure is 0.2Mpa.
[0044] Example 3
[0045] The difference from Example 1 is that when the vulcanizing agent is sprayed, it is sprayed 3 times during the melting period, each time for 5 minutes, and after stopping the feeding, it enters the vulcanization period. During the vulcanization period, the vulcanizing agent is sprayed intermittently 5 times by a spray gun, each time for 10 minutes. The pyrite contains 0.2% water after drying, and the particle size is below 38μm, accounting for 90%, the diameter of the spray gun tuyere is 15mm, and the air delivery pressure is 0.3Mpa.
[0046] The tin content of the final slag, the utilization rate of the sulfiding agent, the energy consumption per ton of tin in the fuming furnace and the SO2 content in the flue gas in Comparative Example 1 and Examples 1 to 3 are shown in Table 1.
[0047] Table 1
[0048] Final slag tin content, wt% Vulcanizing agent utilization, % Energy consumption per ton of tin, kgce <![CDATA[Volume content of SO2 in flue gas, %]]> Comparative Example 1 0.30 45.0 2800 2.5 Example 1 0.15 60.3 2380 2.1 Example 2 0.13 65.2 2300 2.0 Example 3 0.10 67.5 2250 1.8
[0049] By comparing the conventional process example with the new process examples 1 to 3, it can be seen that the use of the process of the present invention can effectively improve the utilization rate of the sulfiding agent, reduce its usage, and reduce energy consumption and SO2 content in flue gas.
[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool, characterized in that: include: Feeding process: adding a mixture of tin-containing material and flux into the fuming furnace through the feeding port of the fuming furnace, and spraying a mixture of pulverized coal and air into the fuming furnace through a first spray gun, so that the tin-containing material is melted to form a molten pool during the heat release of the pulverized coal combustion; during the melting of the tin-containing material, intermittently spraying the dried vulcanizing agent into the molten pool through a second spray gun; Sulfidation reaction process: stop feeding the mixed material, and continue to spray the mixture of pulverized coal and air, and continue to intermittently spray the dried sulfiding agent into the molten pool, so that the tin undergoes a sulfidation reaction under stirring, volatilizes in the form of stannous sulfide, and is oxidized in the flue gas flow at the top of the fuming furnace to form stannous oxide and discharged from the fuming furnace.
2. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to claim 1, characterized in that: During the feeding process, the mixed material is added in batches; when more than half of the total amount of the mixed material has been added to the furnace, the dried vulcanizing agent is intermittently sprayed into the molten pool through the second spray gun.
3. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to claim 2, characterized in that: During the feeding process, the mixture is added in the form of 5 to 20 batches, and the feeding time for each batch is 5 to 20 minutes; when more than half of the total amount of the mixture has been added to the furnace, the dried vulcanizing agent is intermittently sprayed into the molten pool 2 to 3 times through the second spray gun, and each spraying lasts 3 to 5 minutes.
4. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to any one of claims 1 to 3, characterized in that: During the vulcanization reaction, the dried vulcanizing agent is sprayed into the molten pool intermittently 2 to 5 times, and each spraying lasts for 5 to 10 minutes.
5. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to claim 4, characterized in that: The total duration of the feeding process is 0.5 to 1.5 hours, and the total duration of the vulcanization reaction process is 1 to 2 hours.
6. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to any one of claims 1 to 5, characterized in that: The second spray gun is a single-channel spray gun, and the diameter of the spray gun air outlet is 15-25 mm; when the second spray gun sprays the dried vulcanizing agent, nitrogen or air is used as the carrier gas, the spraying pressure is 0.1-0.15 MPa, and the loading amount of the vulcanizing agent is 5-30 kg / Nm 3 The first spray gun is a single-channel spray gun, and the diameter of the spray gun air outlet is 15-25 mm; when the first spray gun sprays the mixture of pulverized coal and air, the spray pressure is 0.1-0.15 MPa, and the load of the pulverized coal is 5-30 kg / Nm 3 .
7. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to claim 6, characterized in that: There are a plurality of the second spray guns, and the plurality of the second spray guns are arranged at equal intervals on the side of the fuming furnace and arranged in the horizontal direction of the fuming furnace; and one first spray gun is arranged between two adjacent second spray guns.
8. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to claim 7, characterized in that: The heights of the first spray gun and the second spray gun from the bottom wall of the fuming furnace are h, and the total height of the furnace body inside the fuming furnace is H, then h / H=1 / 15 to 1 / 5.
9. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to any one of claims 1 to 8, characterized in that: The sulfiding agent is pyrite and / or pyrrhotite; preferably, the particle size of the sulfiding agent is 38 to 74 μm; Preferably, the moisture content of the dried vulcanizing agent is less than 1%.
10. The method for smelting tin-containing materials by spraying a sulfidizing agent in an intermittent molten pool according to any one of claims 1 to 8, characterized in that: The flux is one or more of siliceous flux, calcium flux and iron flux; Preferably, the siliceous flux is one or more of quartz stone, silica, and quartz sand; Preferably, the calcium flux is one or more of quicklime, slaked lime and limestone; Preferably, the iron flux is one or more of iron ore and fumed slag.