360MPa-grade microbial-corrosion-resistant copper-containing antibacterial hot-rolled plate coil and preparation method thereof

By controlling the chemical composition and preparation process, a 360MPa-grade copper-containing antibacterial hot-rolled steel coil resistant to microbial corrosion was prepared, which solved the problem of insufficient corrosion resistance of traditional materials in microbial corrosive environments and achieved high-efficiency antibacterial performance and low-cost mechanical properties.

CN118957423AActive Publication Date: 2024-11-15МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411181159.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively resist microbial corrosion, especially in the service environment of gathering and transmission pipelines, where traditional pipeline steel materials are expensive and lack sufficient corrosion resistance.

Method used

A copper-containing antibacterial hot-rolled steel coil with a microbial corrosion resistance of 360MPa was designed. By controlling the chemical composition and preparation process, including molten iron pretreatment, converter smelting, LF ladle refining, RH vacuum degassing, continuous casting and controlled rolling, polygonal ferrite and acicular ferrite structures were formed. Alloying elements such as Cu, Ti and Ca were added to improve the antibacterial properties.

Benefits of technology

It achieves excellent resistance to microbial corrosion in SRB environments, with low uniform corrosion rate, small maximum pitting depth, good mechanical properties, and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957423A_ABST
    Figure CN118957423A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel production, and discloses a 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled plate coil which comprises the following chemical components in percentage by mass: less than or equal to 0.30% of Si, less than or equal to 0.50% of Mn, less than or equal to 0.010% of P, less than or equal to 0.0020% of S, 1.00-1.85% of Cu, less than or equal to 0.030% of Nb, 0.010-0.020% of Ti, 0.0015-0.0020% of Ca and the balance of Fe and inevitable impurities. The invention further discloses a preparation method of the 360 MPa grade microbial corrosion resistant copper-containing antibacterial hot rolled plate coil. According to the 360MPa-grade microbial-corrosion-resistant copper-containing antibacterial hot-rolled plate coil and the preparation method thereof, the mechanical property is good, and the corrosion resistance is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and in particular to a 360MPa-level microbial corrosion-resistant copper-containing antibacterial hot-rolled coil and a preparation method thereof. Background Art

[0002] Microorganisms attach to the surface of materials and form biofilms. The bacteria in the biofilm can obtain electrons from metals through direct or indirect electron transfer, thus leading to the occurrence of microbial corrosion. Biofilm is the main factor leading to microbial corrosion. The most prominent hazard of microbial corrosion is the local corrosion of materials, which accelerates the progress of corrosion and expands the severity of the hazard. Microbial corrosion exists in the service environment of gathering and transportation pipelines. Traditional pipeline steel materials based on carbon, manganese and micro-alloy elements cannot resist microbial corrosion. Although stainless steel has good corrosion resistance, it is expensive. Summary of the invention

[0003] The purpose of the present invention is to address the deficiencies of the above-mentioned technology and provide a 360MPa-level microbial corrosion-resistant copper-containing antibacterial hot-rolled coil and a preparation method thereof, which has good mechanical properties and strong corrosion resistance.

[0004] To achieve the above-mentioned purpose, the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil designed by the present invention has the following chemical components in percentage by mass: Si≤0.30%, Mn≤0.50%, P≤0.010%, S≤0.0020%, Cu: 1.00-1.85%, Nb≤0.030%, Ti: 0.010-0.020%, Ca: 0.0015-0.0020%, and the rest is Fe and unavoidable impurities.

[0005] Preferably, no carbon element is added, and only the residual carbon introduced when the alloy is added during the smelting process is retained, with a mass percentage of ≤0.03%.

[0006] Preferably, Ni≤0.10%.

[0007] The design principles of the main alloying elements and mass percentages of the present invention are as follows:

[0008] C (carbon): C is the most economical element for improving the strength of steel, but too high a C content will deteriorate the welding performance of the steel and reduce the plasticity and toughness. Therefore, the present invention does not intentionally add carbon elements, and only retains the residual carbon brought in when the alloy is added during the smelting process, and its mass percentage is controlled to be ≤0.03%.

[0009] Mn (manganese): Mn is one of the important solid solution strengthening elements in steel and an important deoxidizing element in the steelmaking process. Mn can also improve the stability of austenite, expand the austenite phase region, and promote the transformation of bainite structure. However, too high Mn content will not only increase the manufacturing cost, but also deteriorate the welding performance and corrosion resistance of the steel. Therefore, its content is designed to be ≤0.50%.

[0010] Cu (copper): Cu can significantly improve the atmospheric corrosion resistance of the material, but the melting point of Cu is relatively low, only 1083°C. Too high a content of Cu can easily lead to steel leakage during continuous casting and edge cracks during hot rolling. Therefore, the mass percentage of Cu is controlled to be 1.00-1.85%.

[0011] Ni (nickel): Ni can increase the self-corrosion potential of the material, reduce the corrosion tendency, improve the atmospheric corrosion resistance, and react with Cu to form a high melting point Cu-Ni binary alloy phase, effectively preventing copper embrittlement caused by Cu. However, Ni is a precious metal element, and excessive content significantly increases the cost of steel manufacturing. Therefore, the Ni content is controlled at ≤0.10% and is not deliberately added.

[0012] Ti (titanium): Ti is a strong nitride-forming element and suppresses the coarsening of austenite grains during heating.

[0013] Ca (Calcium): Promotes the spheroidization of non-metallic inclusions, helps improve the material's resistance to atmospheric corrosion, and improves the material's low-temperature toughness. The content is controlled at 0.0015-0.0020%.

[0014] P (Phosphorus): Although P improves the corrosion resistance of steel, it reduces the low-temperature toughness of steel and increases the sensitivity of welding cracks, so it is controlled within 0.010%.

[0015] S (sulfur): S is a harmful residual element in steel. It is easy to react with Mn to form MnS non-metallic inclusions, which reduces the atmospheric corrosion resistance. Therefore, it is controlled within 0.0020%.

[0016] A method for preparing a 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil comprises the following steps: molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting → slab heating → controlled rolling → controlled cooling → coiling, wherein the molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting adopts clean steel smelting technology, passes through an LF furnace, an RH furnace and undergoes calcium treatment to control the number, shape and size of non-metallic inclusions and reduce the formation of non-metallic inclusions, and the controlled rolling includes rough rolling and finish rolling, and multiple rolling passes are performed in the austenite recrystallization zone during the rough rolling stage.

[0017] Preferably, the slab heating temperature is 1200-1300°C.

[0018] Preferably, the thickness of the rolled piece after rough rolling is controlled at 45 to 60 mm.

[0019] Preferably, the start temperature of finishing rolling is controlled at 1000-1060°C, and the final temperature of finishing rolling is controlled at 850-890°C.

[0020] Preferably, the coiling temperature is controlled at 620-680°C.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. Good mechanical properties, strong corrosion resistance and low cost;

[0023] 2. The microstructure is mainly composed of polygonal ferrite and acicular ferrite, and the grain size is 10 to 12 levels;

[0024] 3. Mechanical properties: Rt0.5: 360~500MPa, Rm: 460~600MPa, -20℃ impact energy ≥150J;

[0025] 4. Resistance to microbial corrosion: After testing for 168 hours in an environment with an SRB concentration of 25,000 / ml, the uniform corrosion rate is ≤0.22mm / a and the maximum pitting depth is ≤2.8μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a microstructural morphology diagram of the 360MPa-level microbial corrosion-resistant copper-containing antibacterial hot-rolled coil of the present invention under an optical microscope. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] A 360MPa-level microbial corrosion-resistant copper-containing antibacterial hot-rolled coil, the chemical components of which are as follows by mass percentage: Si≤0.30%, Mn≤0.50%, P≤0.010%, S≤0.0020%, Cu: 1.00-1.85%, Nb≤0.030%, Ti: 0.010-0.020%, Ca: 0.0015-0.0020%, and the rest is Fe and unavoidable impurities.

[0029] Among them, no carbon element is added, and only the residual carbon brought in when the alloy is added during the smelting process is retained, with a mass percentage of ≤0.03%. In addition, Ni is ≤0.10%.

[0030] The preparation method of the above-mentioned 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil comprises the following steps: molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting → slab heating → controlled rolling → controlled cooling → coiling, wherein the molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting adopts clean steel smelting technology, passes through LF furnace, RH furnace and calcium treatment, and the controlled rolling includes rough rolling and finish rolling, and multiple rolling passes are carried out in the austenite recrystallization zone during the rough rolling stage.

[0031] In addition, the slab heating temperature is 1200-1300°C, the thickness of the rolled piece after rough rolling is controlled at 40-60mm, the start temperature of finishing rolling is controlled at 1000-1060°C, the final rolling temperature of finishing rolling is controlled at 850-890°C, and the coiling temperature is controlled at 620-680°C.

[0032] Ten groups of examples are listed to illustrate the implementation of this process, as shown in Table 1, which is a chemical composition table of the ten examples:

[0033] Table 1 Chemical composition of each example (wt%)

[0034] C Si Mn P S Cu Ni Nb Ti Ca Example 1 0.023 0.24 0.37 0.0100 0.0004 1.14 0.10 0.022 0.017 0.0016 Example 2 0.020 0.22 0.42 0.0082 0.0012 1.68 0.08 0.026 0.015 0.0015 Example 3 0.025 0.23 0.50 0.0046 0.0008 1.24 0.06 0.018 0.012 0.0017 Example 4 0.021 0.28 0.32 0.0054 0.0014 1.37 0.07 0.030 0.016 0.0016 Example 5 0.030 0.21 0.41 0.0064 0.0016 1.49 0.06 0.022 0.020 0.0018 Example 6 0.019 0.26 0.29 0.0071 0.0004 1.85 0.09 0.016 0.018 0.0018 Example 7 0.016 0.30 0.35 0.0051 0.0009 1.16 0.05 0.018 0.014 0.0016 Example 8 0.025 0.23 0.41 0.0042 0.0020 1.00 0.04 0.026 0.010 0.0020 Example 9 0.023 0.25 0.35 0.0054 0.0015 1.75 0.06 0.024 0.015 0.0017 Example 10 0.024 0.22 0.31 0.0034 0.0018 1.65 0.04 0.028 0.014 0.0017

[0035] As shown in Table 2, the rolling process parameters of 10 embodiments are as follows:

[0036] Table 2 Main process parameters of rolling process of each embodiment

[0037]

[0038]

[0039] As shown in Table 3, the mechanical properties of 10 embodiments are as follows:

[0040] Table 3 Mechanical properties of each embodiment (I)

[0041]

[0042] As shown in Table 4, the Charpy impact properties of 10 embodiments are shown, wherein the impact energy specimen size of embodiments 1 to 5 is 5×10×55, and the impact energy specimen size of embodiments 6 to 10 is 10×10×55. Each embodiment is tested three times and the average value is taken:

[0043] Table 4 Charpy impact energy performance of each embodiment

[0044]

[0045] The microbial corrosion resistance behavior of the steel plate of the embodiment of the present invention was studied in an environment containing sulfate reducing bacteria (SRB) to observe the shape of corrosion pits and uniform corrosion rate. The embodiment achieved the target performance at a relatively low cost.

[0046] As shown in Table 5, the antibacterial properties of 10 embodiments are shown:

[0047] Table 5 Antibacterial properties of each embodiment

[0048]

[0049] It can be seen from the embodiments in the above table that the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil of the present invention has the following mechanical properties: Rt0.5: 360-500MPa, Rm: 460-600MPa, -20°C impact energy ≥ 150J (wherein the impact energy sample size of Examples 1-5 is 5×10×55, and the impact energy conversion needs to be multiplied by 2); when the SRB concentration is 25000 / ml, its uniform corrosion rate is ≤0.22mm / a, and the maximum pitting pit depth is ≤2.8μm, with good mechanical properties, strong corrosion resistance, and low cost. In addition, Figure 1 As shown, the microstructure is acicular ferrite + quasi-polygonal ferrite, and the grain size ranges from 10 to 12 levels.

[0050] It should be noted that the description of the above technical solutions is exemplary, and this specification can be embodied in different forms and should not be interpreted as being limited to the technical solutions set forth herein. On the contrary, providing these descriptions will make the disclosure of the present invention thorough and complete, and will fully convey the scope disclosed in this specification to those skilled in the art. In addition, the technical solutions of the present invention are limited only by the scope of the claims.

[0051] The various aspects disclosed for describing the present specification and claims are merely examples, and therefore, the present specification and claims are not limited to the details shown. In the above description, when the detailed description of the related known functions or configurations is determined to be unnecessary to obscure the focus of the present specification and claims, the detailed description will be omitted.

[0052] In the case of using “including”, “having” and “comprising” described in the present specification, unless otherwise used, there may also be another part or other parts, and the terms used may generally be in the singular but may also represent the plural form.

[0053] Finally, it should be pointed out that the above content is a further detailed description of the invention in combination with specific implementation methods. It cannot be considered that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, simple replacements made without departing from the concept of the present invention should be regarded as belonging to the protection scope of the present invention. The above embodiments are only more representative examples of the present invention. Obviously, the present invention is not limited to the above embodiments, and there can be many variations. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention should be considered to belong to the protection scope of the present invention.

[0054] At the same time, it should be noted that the description of the above technical solutions is exemplary, and this specification can be embodied in different forms and should not be construed as being limited to the technical solutions set forth herein. On the contrary, providing these descriptions will make the disclosure of the present invention thorough and complete, and will fully convey the scope disclosed in this specification to those skilled in the art. In addition, the technical solutions of the present invention are limited only by the scope of the claims. The features of the various embodiments of the present invention may be partially or completely combined or spliced ​​with each other, and may be performed in various different configurations as those skilled in the art may fully understand. The embodiments of the present invention may be performed independently of each other, or may be performed together in a mutually dependent relationship.

[0055] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, and the above structures should be regarded as belonging to the protection scope of the present invention.

Claims

1. A 360MPa grade microbial corrosion resistant copper-containing antibacterial hot-rolled coil, characterized in that: The mass percentage of its chemical composition is: Si≤0.30%, Mn≤0.50%, P≤0.010%, S≤0.0020%, Cu: 1.00~1.85%, Nb≤0.030%, Ti: 0.010~0.020%, Ca: 0.0015~0.0020%, and the rest is Fe and unavoidable impurities.

2. The 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 1, characterized in that: No carbon element is added, only the residual carbon brought in when the alloy is added during the smelting process is retained, with a mass percentage of ≤0.03%.

3. The 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 1, characterized in that: Ni≤0.10%.

4. A method for preparing the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil as claimed in claim 1, characterized in that: The process comprises the following steps: molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting → slab heating → controlled rolling → controlled cooling → coiling, wherein the process of molten iron pretreatment → converter smelting → LF refining → RH vacuum degassing → continuous casting adopts clean steel smelting technology, passes through LF furnace, RH furnace and calcium treatment, and the controlled rolling includes rough rolling and finish rolling, and multiple rolling passes are carried out in the austenite recrystallization zone during the rough rolling stage.

5. The method for preparing the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 4, characterized in that: The slab heating temperature is 1200-1300°C.

6. The method for preparing the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 4, characterized in that: The thickness of the rolled piece after rough rolling is controlled at 40-60 mm.

7. The method for preparing the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 4, characterized in that: The start temperature of finishing rolling is controlled at 1000-1060°C, and the final temperature of finishing rolling is controlled at 850-890°C.

8. The method for preparing the 360MPa-grade microbial corrosion-resistant copper-containing antibacterial hot-rolled coil according to claim 4, characterized in that: The coiling temperature is controlled at 620-680°C.

Citation Information

Patent Citations

  • Highly stable, steel and steel strips or steel sheets cold-formed, method for the production of steel strips and uses of said steel

    CA2414138A1

  • Thick steel plate with high strength and toughness as well as uniform performance in thickness direction and production method of thick steel plate

    CN103667921A

  • X80-grade pipeline steel plate with seawater corrosion resistance and large deformation resistance and manufacturing method thereof

    CN111961957A

  • Microbial corrosion resistant pipeline steel with yield strength of 480 MPa and preparation method thereof

    CN115449698A

  • Corrosion-resistant steel for ship superstructure

    KR1020120085674A