HRB600E reinforcing steel bar with impact energy greater than or equal to 27J at low temperature of-20 DEG C and production method and application thereof
By controlling chemical composition and metallographic structure, HRB600E steel bars with impact power value of more than 27J under low temperature environment -20℃ were prepared, which solved the problem of insufficient impact power of existing high-strength steel bars in low temperature environments and ensured that the steel bars were in cold environments and meet the mechanical properties and metallographic structure requirements of national standards.
Patent Information
- Application Number
- CN202411066329.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The impact power of the existing 600MPa high-strength steel bars in low temperature environments is insufficient, and cannot meet the bending processing requirements below -20℃, and the existing standards have missing requirements for low-temperature impact power.
By controlling the chemical composition and metallographic structure, 0.25%≤C≤0.28%, 0.60%≤Si≤0.80%, 1.40%≤Mn≤1.60%, 0.110%≤V≤0.130%, 0.01%≤Nb≤0.03% were prepared , HRB600E steel bars with 0.020%≤N≤0.030%, P≤0.020%, S≤0.030%, and steelmaking, LF refining, continuous casting, heating and rolling steps are used to ensure that the steel bars are at -20℃ The impact power value reaches more than 27J.
The normal bending processing capability of HRB600E steel bars in low temperature environment -20℃ has been achieved, and it meets the mechanical properties and metallographic structure requirements of GB/T 1499.2-2018 standards.
Smart Images

Figure CN118957433A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of HRB600E steel bar production, and in particular to a HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, and a production method and application thereof. Background Art
[0002] In recent years, with the promotion and use of high-strength steel bars, the production and application of 600MPa high-strength steel bars have increased year by year, and how to efficiently and stably produce high-strength steel bars has attracted much attention. The GB / T 1499.2-2018 standard has clear index requirements for chemical composition, mechanical properties and metallographic structure, but for impact energy, currently only YB-T4364-2014 "Hot-rolled ribbed steel bars for anchor rods" has requirements for room temperature impact values. Because the requirements for composition and seismic performance of this standard are different from those of GB / T 1499.2-2018, it can be used as a reference for impact energy comparison. Among some currently disclosed 600MPa high-plasticity anchor rod steel bars, the mechanical properties and metallographic structure of the steel bars meet the GB / T1499.2-2018 standard, and their impact energy at room temperature is not less than 100J. Summary of the invention
[0003] In order to solve the above problems, the present application proposes a HRB600E steel bar with a low-temperature impact energy of ≥27J at -20℃ and a production method and application thereof. The HRB600E steel bar prepared by the production method has an impact energy of more than 27J at -20℃, ensuring that the steel bar can be normally bent and processed in a cold environment above -20℃.
[0004] This application is implemented through the following technical solutions:
[0005] One of the purposes of the present application is to provide a HRB600E steel bar with a low-temperature impact energy of -20°C ≥27J, wherein the HRB600E steel bar includes iron and the following components by weight: 0.25%≤C≤0.28%, 0.60%≤Si≤0.80%, 1.40%≤Mn≤1.60%, 0.110%≤V≤0.130%, 0.01%≤Nb≤0.03%, 0.020%≤N≤0.030%, P≤0.020%, and S≤0.030%.
[0006] The HRB600E steel bar provided in the present application has a yield strength of 620MPa-680MPa, a tensile strength of 780MPa-860MPa, a strength-to-yield ratio of 1.25-1.30, a maximum force total elongation of 9.0%-12.0%, and an impact energy value of more than 27J at a low temperature of -20°C, which ensures that the steel bar can be normally bent and processed in a cold environment above -20°C.
[0007] In some possible implementations, the HRB600E steel bar is composed of the following components in weight fractions: 0.25%≤C≤0.28%, 0.60%≤Si≤0.80%, 1.40%≤Mn≤1.60%, 0.110%≤V≤0.130%, 0.01%≤Nb≤0.03%, 0.020%≤N≤0.030%, P≤0.020%, S≤0.030%, and the remainder is iron and unavoidable impurities.
[0008] In some possible implementations, the HRB600E steel bar includes iron and also includes the following components in weight fractions: 0.27%≤C≤0.28%, 0.66%≤Si≤0.72%, 1.52%≤Mn≤1.56%, 0.115%≤V≤0.128%, 0.016%≤Nb≤0.020%, 0.024%≤N≤0.027%, 0.016%≤P≤0.018% and 0.020%≤S≤0.030%.
[0009] In some possible implementations, the HRB600E steel bar is composed of the following components in weight fractions: 0.27%≤C≤0.28%, 0.66%≤Si≤0.72%, 1.52%≤Mn≤1.56%, 0.115%≤V≤0.128%, 0.016%≤Nb≤0.020%, 0.024%≤N≤0.027%, 0.016%≤P≤0.018% and 0.020%≤S≤0.030%, with the remainder being iron and unavoidable impurities.
[0010] In some possible implementations, the HRB600E steel bar includes iron and the following components by weight: 0.28% C, 0.72% Si, 1.56% Mn, 0.115% V, 0.020% Nb, 0.024% N, 0.018% P, and 0.020% S. In this case, the carbon equivalent of the HRB600E steel bar is 0.57%, which meets the requirements of the national standard GB / T 1499.2-2018 for the carbon equivalent of steel bars (0.58%).
[0011] In some possible implementations, the HRB600E steel bar includes iron and the following components by weight: 0.27% C, 0.66% Si, 1.55% Mn, 0.122% V, 0.018% Nb, 0.026% N, 0.016% P, and 0.025% S. In this case, the carbon equivalent of the HRB600E steel bar is 0.56%, which meets the requirements of the national standard GB / T 1499.2-2018 for the carbon equivalent of steel bars (0.58%).
[0012] In some possible implementations, the HRB600E steel bar includes iron and the following components by weight: 0.27% C, 0.68% Si, 1.52% Mn, 0.128% V, 0.016% Nb, 0.027% N, 0.018% P, and 0.030% S. In this case, the carbon equivalent of the HRB600E steel bar is 0.55%, which meets the requirements of the national standard GB / T 1499.2-2018 for the carbon equivalent of steel bars (0.58%).
[0013] In some possible implementations, the metallographic structure of the HRB600E steel bar includes a mixed structure of ferrite and pearlite. In terms of area ratio, the ferrite accounts for 55% to 62%, and the pearlite accounts for 38% to 45%. In this case, the impact energy value of the HRB600E steel bar at a low temperature of -20°C is greater than 27J.
[0014] In some possible implementations, the diameter of the HRB600E steel bar is 16 mm to 32 mm.
[0015] The second object of the present application is to provide a method for producing HRB600E steel bars with a low-temperature impact energy of ≥27J at -20°C provided in the present application, comprising the following steps:
[0016] The raw materials are subjected to steps including steelmaking, LF refining, continuous casting, heating and rolling to obtain HRB600E steel bars.
[0017] In the production method of HRB600E steel bars of the present application, the steelmaking and LF refining are combined to control the content of P and S in the HRB600E steel bars; the added Si and Mn have a strengthening effect and a fine grain effect, and the Nb content is controlled to improve the grain size of the structure and the toughness of the HRB600E steel bar material. The HRB600E steel bars produced by the production method have a smooth surface, and the yield strength, tensile strength, strength-to-yield ratio and maximum force total elongation meet the standards. In addition, the impact energy value of the HRB600E steel bars produced at a low temperature of -20°C is above 27J.
[0018] In some possible implementations, the heating temperature is 1100° C. to 1200° C., and the tapping temperature is 1020° C. to 1080° C. At this heating temperature and tapping temperature, the alloy elements in the steel can be fully dissolved, while preventing grain coarsening caused by high heating temperature.
[0019] In some possible implementations, in the rolling step, the temperature of the upper cooling bed is 920° C. to 980° C. At this temperature, it can be ensured that the microalloys are fully precipitated during the cooling after rolling and the metallographic structure is qualified.
[0020] The third object of the present application is to provide an application of the HRB600E steel bar provided by the present application or the HRB600E steel bar produced by the production method provided by the present application in the field of low temperature environment engineering and / or earthquake resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0022] Figure 1 Schematic diagram of the metallographic structure of the steel bar 500X of ∮16 in Example 1 of the present application;
[0023] Figure 2 Schematic diagram of the metallographic structure of the steel bar 500X of ∮22 in Example 2 of the present application;
[0024] Figure 3 This is a schematic diagram of the metallographic structure of the steel bar 500X ∮32 in Example 3 of the present application.
[0025] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0027] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0028] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0029] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0030] Example 1
[0031] Embodiment 1 proposes a HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, which is composed of the following components in weight fractions: 0.28% C, 0.72% Si, 1.56% Mn, 0.115% V, 0.020% Nb, 0.024% N, 0.018% P, 0.020% S, and the rest is iron and unavoidable impurities.
[0032] Example 1 also provides a method for producing the HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, comprising the following steps: the raw materials are subjected to steelmaking, LF refining, continuous casting, heating and rolling steps to obtain the HRB600E steel bar.
[0033] The heating temperature is 1100℃~1200℃, the tapping temperature is 1045℃, and during the rolling step, the temperature of the upper cooling bed is 940℃. The diameter of the produced steel bar is 16mm.
[0034] Example 2
[0035] Example 2 proposes a HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, which is composed of the following components in weight fractions: 0.27% C, 0.66% Si, 1.55% Mn, 0.122% V, 0.018% Nb, 0.026% N, 0.016% P, 0.025% S, and the rest is iron and unavoidable impurities.
[0036] Example 2 also proposes a production method for the HRB600E steel bar with a low-temperature impact energy of -20°C ≥27J, comprising the following steps: the raw materials are subjected to steelmaking, LF refining, continuous casting, heating and rolling steps to obtain the HRB600E steel bar.
[0037] The heating temperature is 1100℃~1200℃, the tapping temperature is 1050℃, and during the rolling step, the temperature of the upper cooling bed is 950℃. The diameter of the produced steel bar is 22mm.
[0038] Example 3
[0039] Example 3 proposes a HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, which is composed of the following components in weight fractions: 0.27% C, 0.66% Si, 1.52% Mn, 0.128% V, 0.016% Nb, 0.027% N, 0.018% P, 0.030% S, and the rest is iron and unavoidable impurities.
[0040] Example 3 also proposes a production method for HRB600E steel bar with -20°C low-temperature impact energy ≥ 27J, comprising the following steps: raw materials are subjected to steelmaking, LF refining, continuous casting, heating and rolling steps to obtain HRB600E steel bar.
[0041] The heating temperature is 1100℃~1200℃, the tapping temperature is 1050℃, and during the rolling step, the temperature of the upper cooling bed is 960℃. The diameter of the produced steel bar is 32mm.
[0042] In order to verify the progress of the HRB600E steel bars and the production method of HRB600E steel bars provided in the examples of the present application, the HRB600E steel bars provided in Examples 1 to 3 (the components and contents are shown in Table 1 below) were respectively tested for tensile strength (R o m ), lower yield strength (R o el ), flexion-to-flexion ratio (R o el / R el ), strength-to-yield ratio (R o m / R o el ), elongation after fracture (A) and total elongation at maximum force (A gt ) test, and the test results are shown in Table 2 below; according to GB / T 229-2020, the samples were tested for low-temperature impact energy at -20°C, and the test results are shown in Table 3 below; according to standard GB / T 1499.2-2018, the grain size and metallographic structure of the samples were tested, and the results are shown in Table 4 below.
[0043] Table 1
[0044] C(%) Si(%) Mn(%) V(%) Nb(%) N(%) P(%) S(%) Ceq (%) Example 1 0.28 0.72 1.56 0.115 0.020 0.024 0.018 0.020 0.57 Example 2 0.27 0.66 1.55 0.122 0.018 0.026 0.016 0.025 0.56 Example 3 0.27 0.66 1.52 0.128 0.016 0.027 0.018 0.030 0.55
[0045] Table 2
[0046]
[0047] Table 3
[0048]
[0049] Table 4
[0050]
[0051] From Tables 1 to 4 above and the instructions Figures 1 to 3 At least the following conclusions can be drawn:
[0052] The component content of the HRB600E steel bar in the embodiment of the present application complies with the GB / T 1499.2-2018 standard, and the impact energy is 27J to 42J in a low temperature environment of -20°C.
[0053] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C, the HRB600E steel bar comprising iron, characterized in that: It also includes the following components in weight fractions: 0.25%≤C≤0.28%, 0.60%≤Si≤0.80%, 1.40%≤Mn≤1.60%, 0.110%≤V≤0.130%, 0.01%≤Nb≤0.03%, 0.020%≤N≤0.030%, P≤0.020%, and S≤0.030%.
2. The HRB600E steel bar with a low-temperature impact energy of -20°C ≥ 27J according to claim 1, characterized in that: The HRB600E steel bar includes iron and the following components in weight fractions: 0.27%≤C≤0.28%, 0.66%≤Si≤0.72%, 1.52%≤Mn≤1.56%, 0.115%≤V≤0.128%, 0.016%≤Nb≤0.020%, 0.024%≤N≤0.027%, 0.016%≤P≤0.018% and 0.020%≤S≤0.030%.
3. The HRB600E steel bar with -20°C low temperature impact energy ≥ 27J according to claim 1 or 2, characterized in that: The metallographic structure of the HRB600E steel bar includes a mixed structure of ferrite and pearlite.
4. The HRB600E steel bar with -20°C low-temperature impact energy ≥ 27J according to claim 3, characterized in that: In terms of area ratio, the ferrite structure accounts for 55% to 62%, and the pearlite structure accounts for 38% to 45%.
5. The HRB600E steel bar according to claim 1, 2 or 4, characterized in that: The grain size of the HRB600E steel bar is 11 to 13 grades.
6. The HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C according to claim 5, characterized in that: The diameter of the HRB600E steel bar is 16 mm to 32 mm.
7. A method for producing HRB600E steel bars with a low-temperature impact energy of ≥27J at -20°C as claimed in any one of claims 1 to 6, characterized in that: The steps include: The raw materials are subjected to steps including steelmaking, LF refining, continuous casting, heating, rolling and cooling to obtain the HRB600E steel bar.
8. The method for producing HRB600E steel bars with -20°C low-temperature impact energy ≥ 27J according to claim 7, characterized in that: The heating temperature is 1100°C to 1200°C, and the heated steel tapping temperature is 1020°C to 1080°C.
9. The method for producing HRB600E steel bars with -20°C low-temperature impact energy ≥ 27J according to claim 7 or 8, characterized in that: In the cooling step, the temperature of the upper cooling bed is 920°C to 980°C.
10. Use of the HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C as claimed in any one of claims 1 to 7 or the HRB600E steel bar with a low-temperature impact energy of ≥27J at -20°C produced by the production method as claimed in any one of claims 8 to 9 in the field of low-temperature processing and / or earthquake resistance.