A composite multilayer TiAlN / AlTiN / ZrN coated cutting tool and its preparation method
By alternately plating TiAlN, AlTiN, and ZrN layers on titanium alloy cutting tools, the problem of easy coating failure was solved, resulting in coated tools with high wear resistance and high adhesion, which extended tool life and reduced frictional heat.
Patent Information
- Application Number
- CN202411040436.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing titanium alloy cutting tool coatings are prone to failure, resulting in insufficient tool life.
The TiAlN/AlTiN/ZrN coated cutting tool with a composite multilayer structure is produced by alternating TiAlN, AlTiN and ZrN layers on the substrate material through physical vapor deposition. The process parameters are optimized to ensure the adhesion of each layer and a low coefficient of friction.
It improves the wear resistance and adhesion of the coating, reduces coating delamination, extends the cutting life of the tool, reduces the heat generated by friction, and improves cutting efficiency.
Smart Images

Figure CN118957492B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal cutting tool technology, and in particular to a composite multilayer TiAlN / AlTiN / ZrN coated tool and its preparation method. Background Technology
[0002] Titanium alloys are widely used in aerospace, medical, and 3C industries due to their excellent properties such as lightweight, high strength, and corrosion resistance. However, these favorable material properties also present challenges in their machining. The increasingly widespread application of titanium alloys has led to a growing market demand for coatings on titanium alloy cutting tools.
[0003] There is a lot of research on coatings for titanium alloy machining. One of them is to use physical vapor deposition (PVD) technology to coat the tool surface with TiAlN coating material, which has high hardness, high chemical stability, low friction, wear resistance and high temperature resistance, thereby improving cutting efficiency and extending cutting life.
[0004] To further improve the coating's performance, a high-hardness AlTiN coating is applied on top of the TiAlN coating. This high-Al content coating increases the content of high-hardness Al2O3. Patent document CN202310021859.X discloses a multi-structure heterogeneous coating, its preparation method, and its applications. This coating comprises a TiAlN base layer, an AlTiN gradient layer with increasing Al content, an AlTiN / TiSiN nanolayer, and a TiSiN nanocomposite layer, sequentially connected. This coating exhibits strong toughness and corrosion resistance, and high adhesion. The cutting life of tools coated with this coating is significantly longer than that of traditional AlTiN-coated tools. However, the high-hardness AlTiN coating still possesses considerable internal stress, which can affect the service life of coated tools in practical applications. Summary of the Invention
[0005] In view of this, the purpose of this invention is to propose a composite multilayer TiAlN / AlTiN / ZrN coated cutting tool and its preparation method, so as to solve the problem of insufficient tool life caused by easy failure of coatings on titanium alloy cutting tools in the prior art.
[0006] To achieve the above objectives, the present invention provides a composite multilayer TiAlN / AlTiN / ZrN coated cutting tool, comprising a substrate material and multiple material layers deposited on the surface of the substrate material by a PVD process, wherein the first material layer is a TiAlN layer; the second material layer is an AlTiN layer; the third material layer is a ZrN layer; the fourth material layer is an AlTiN layer; the fifth material layer is a ZrN layer; the sixth material layer is an AlTiN layer; and the seventh material layer is a ZrN layer.
[0007] Preferably, the first material layer includes a plurality of bonding layers arranged in a stacked manner, namely a first bonding layer, a second bonding layer and a third bonding layer.
[0008] Preferably, the thickness of the first material layer is between 1.0 and 1.2 μm, and the thickness of the second material layer is between 0.8 and 1.0 μm.
[0009] Furthermore, the present invention also provides a method for preparing a TiAlN / AlTiN / ZrN coated cutting tool with a composite multilayer structure, the specific preparation steps of which are as follows:
[0010] (1) Place the substrate material in the vacuum coating equipment and adjust the vacuum level of the equipment to 8×10. -5 mbar, heat for 60 minutes to raise the temperature to 460-480℃;
[0011] (2) A first material layer is deposited on the substrate material using PVD process. The first material layer is a TiAlN layer.
[0012] (3) A second material layer is deposited on the side of the first material layer away from the substrate material using PVD process. The second material layer is an AlTiN layer.
[0013] (4) A third material layer is deposited on the side of the second material layer away from the substrate material using PVD process. The third material layer is a ZrN layer.
[0014] (5) A fourth material layer is deposited on the side of the third material layer away from the substrate material using PVD process. The fourth material layer is an AlTiN layer.
[0015] (6) A fifth material layer is deposited on the side of the fourth material layer away from the substrate material using PVD process. The fifth material layer is a ZrN layer.
[0016] (7) A sixth material layer is deposited on the side of the fifth material layer away from the substrate material using PVD process. The sixth material layer is an AlTiN layer.
[0017] (8) A seventh material layer is deposited on the side of the sixth material layer away from the substrate material using PVD process. The seventh material layer is a ZrN layer.
[0018] Preferably, the matrix material in step (1) is a cemented carbide.
[0019] Preferably, in step (2), the first material layer comprises multiple stacked bonding layers, and the specific preparation steps are as follows: each bonding layer is deposited sequentially using PVD process. When depositing a single bonding layer, the TiAl target is placed at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1The process is carried out in a nitrogen environment at 480℃ for a preset time with an arc current of 150A, a preset bias voltage, and a flow rate of 1200SCCM. The molar ratio of Ti to Al in the TiAl target is 50 / 50. The bias voltage required during coating is greater for the bonding layer closer to the second material layer.
[0020] Preferably, when the first bonding layer is deposited on the substrate material using the PVD process, the required bias voltage is 40V and the processing time is 40±2min; when the second bonding layer is deposited on the substrate material, the required bias voltage is 80V and the processing time is 2min; when the third bonding layer is deposited on the substrate material, the required bias voltage is 120V and the processing time is 30±2min.
[0021] Preferably, the method for depositing the second material layer in step (3) is as follows: placing the TiAl target and the Al target respectively in a molecular pump with a frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1 The second material layer can be formed on the substrate material by treating it in a nitrogen environment with mbar, arc current of 150A, bias voltage of 80V and temperature of 480℃ for 2 minutes. The N2 flow rate is 1200SCCM. The molar ratio of Ti to Al in the TiAl target is 50 / 50.
[0022] Preferably, the method for depositing the third material layer in step (4) is as follows: placing the Zr target at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1 The third material layer can be formed on the substrate material by treating it in a nitrogen environment with mbar, arc current of 150A, bias voltage of 120V, and temperature of 480℃ for 30 minutes, with an N2 flow rate of 1200SCCM.
[0023] Preferably, the method of depositing AlTiN layer using PVD process in steps (4) and (6) is the same as in step (2); the method of depositing ZrN layer using PVD process in steps (3) and (5) is the same as in step (3).
[0024] The beneficial effects of this invention are:
[0025] (1) The coated cutting tool obtained by the PVD process for depositing ZrN layer has low affinity with the material being processed (titanium alloy). The low affinity makes the wear form of the cutting tool abrasive wear during cutting, and the coating is not easily carried away by the abrasive particles.
[0026] (2) The AlTiN coated cutting tool obtained by the PVD process of this invention has excellent high temperature resistance, red hardness and oxidation resistance, which makes the coating service life longer, improves the wear resistance and adhesion of the coating, makes the coating less prone to failure, avoids coating peeling, and improves the cutting life of the cutting tool.
[0027] (3) The coated cutting tool obtained by the present invention using PVD process to alternately deposit AlTiN layer and ZrN layer has excellent bonding force between AlTiN and ZrN, ensuring that no film delamination occurs during the cutting process. At the same time, it brings a low coefficient of friction. The low coefficient of friction helps to reduce the heat generated by friction between the cutting tool and the workpiece, thereby reducing the heat that extends to the substrate material. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only for this invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0029] Figure 1 This is a partially enlarged cross-sectional view of the cutting tool prepared according to an embodiment of the present invention;
[0030] Figure 2 EDS analysis image of the coating of the cutting tool prepared according to an embodiment of the present invention;
[0031] The diagram is marked as follows:
[0032] 1. Substrate material; 2. First material layer TiAlN coating; 3. Second material layer AlTiN coating; 4. Third material layer ZrN coating; 5. Fourth material layer AlTiN coating; 6. Fifth material layer ZrN coating; 7. Sixth material layer AlTiN coating; 8. Seventh material layer ZrN coating. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.
[0034] As shown in the figure, this embodiment discloses a composite multilayer TiAlN / AlTiN / ZrN coated cutting tool, including a substrate material 1, which is a cemented carbide. Specifically, the substrate material 1 in this embodiment is used for cutting tools made of cemented carbide and high-speed steel, including inserts, end mills, drills, reamers, etc. A first material layer 2 is deposited on the outer side of the substrate material using a PVD process. The first material layer is a TiAlN layer and also includes three bonding layers (not shown in the figure). The thickness of the first material layer is between 1.0 and 1.2 μm. A second material layer 3, which is an AlTiN layer, is deposited on the side of the first material layer 2 away from the substrate material using a PVD process. The thickness of the second material layer 3 is between 0.8 and 1.0 μm. A third material layer 4 is deposited on the side of the second material layer 3 away from the substrate material using a PVD process. The third material layer 4 is a ZrN layer; a fourth material layer 5, which is an AlTiN layer, is deposited on the side of the third material layer 4 away from the substrate material using a PVD process; a fifth material layer 6, which is a ZrN layer, is deposited on the side of the fourth material layer 5 away from the substrate material using a PVD process; a sixth material layer 7, which is an AlTiN layer, is deposited on the side of the fifth material layer 6 away from the substrate material using a PVD process; and a seventh material layer 8, which is a ZrN layer, is deposited on the side of the sixth material layer 7 away from the substrate material using a PVD process.
[0035] Example: A method for preparing a composite multilayer TiAlN / AlTiN / ZrN coated cutting tool, specifically including the following steps:
[0036] (1) Place the cemented carbide in a vacuum coating equipment and adjust the vacuum level of the equipment to 8×10⁻⁶. -5 mbar, heated for 60 minutes, raising the temperature to 470℃;
[0037] (2) A first material layer is deposited on the cemented carbide using PVD process. The first material layer is a TiAlN layer.
[0038] (3) A second material layer is deposited on the side of the first material layer away from the cemented carbide using PVD process. The second material layer is an AlTiN layer.
[0039] (4) A third material layer is deposited on the side of the second material layer away from the cemented carbide using PVD process. The third material layer is a ZrN layer.
[0040] (5) A fourth material layer is deposited on the side of the third material layer away from the cemented carbide using PVD process. The fourth material layer is an AlTiN layer.
[0041] (6) A fifth material layer is deposited on the side of the fourth material layer away from the cemented carbide using PVD process. The fifth material layer is a ZrN layer.
[0042] (7) A sixth material layer is deposited on the side of the fifth material layer away from the cemented carbide using PVD process. The sixth material layer is an AlTiN layer.
[0043] (8) A seventh material layer is deposited on the side of the sixth material layer away from the cemented carbide using PVD process. The seventh material layer is a ZrN layer.
[0044] In step (2), the first material layer comprises multiple stacked bonding layers. The specific preparation steps are as follows: each bonding layer is deposited sequentially using PVD technology. When depositing a single bonding layer, the TiAl target is placed at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1 The process involves a nitrogen atmosphere at 480℃ and a preset time, with an arc current of 150A, a preset bias voltage, and a flow rate of 1200 SCCM. The molar ratio of Ti to Al in the TiAl target is 50 / 50. Specifically, when the first bonding layer is deposited onto the substrate using PVD, the required bias voltage is 40V and the processing time is 40 minutes; when the second bonding layer is deposited onto the substrate, the required bias voltage is 80V and the processing time is 2 minutes; and when the third bonding layer is deposited onto the substrate, the required bias voltage is 120V and the processing time is 30 minutes.
[0045] The method for depositing the second material layer in step (3) involves placing the TiAl target and the Al target at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶, respectively. -1 The second material layer can be formed on the substrate material by treating it in a nitrogen environment with mbar, arc current of 150A, bias voltage of 80V and temperature of 480℃ for 2 minutes. The N2 flow rate is 1200SCCM. The molar ratio of Ti to Al in the TiAl target is 50 / 50.
[0046] The method for depositing the third material layer in step (4) involves placing the Zr target at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1 The third material layer can be formed on the substrate material by treating it in a nitrogen atmosphere with an mbar, an arc current of 150A, a bias voltage of 120V, and a temperature of 480℃ for 30 minutes, wherein the N2 flow rate is 1200SCCM.
[0047] The methods for depositing the AlTiN layer in steps (5) and (7) are the same as those for depositing the AlTiN layer in step (3).
[0048] The method for depositing the AlTiN layer in steps (6) and (8) is the same as the method for depositing the AlTiN layer in step (4).
[0049] It should be noted that this invention is not simply a combination of TiAlN, AlTiN, and ZrN. This patent application focuses on a tool coating developed for machining titanium alloys. The selected coating structure and target material fully consider the machining characteristics of titanium alloys, and the coating has undergone rigorous internal testing. Specifically, the effectiveness of different target materials (structures) is influenced by many factors, such as deposition temperature, magnetic field parameters, cathode, bias voltage, gas flow rate, and ion source. Different parameters produce completely different effects.
[0050] The challenges of bonding AlTiN and ZrN lie in the following three aspects: First, achieving excellent bonding strength between AlTiN and ZrN to ensure that no delamination occurs during tool cutting; second, reducing the droplets of AlTiN and ZrN deposited by arc deposition and lowering the coefficient of friction by optimizing process parameters; and third, controlling the deposition time of each coating layer to achieve the optimal combination of cutting edge sharpness, low coefficient of friction, and coating wear resistance while ensuring that the cutting edge of the tool does not delaminate.
[0051] A series of performance tests were conducted on the coated cutting tools obtained in the examples:
[0052] The coating adhesion was measured using the scratch method, and an automatic scratch tester was used in this experiment. The loading speed was 100 N / m, the scratch length was 5 mm, and the final load was 100 N. Nanohardness was measured using a UNHT nanoindenter with the following parameters: maximum load 10 mN, loading rate 20 mN / min, unloading rate 20 mN / min, and holding time 10 s. Cutting force was measured using a Swiss Kistler 9257B force measuring device at a cutting speed of 105 m / min. The measurement standard was to continuously measure the feed distance twice for each set of inserts under each set of cutting parameters, with each feed distance L = 110 mm. Wear resistance was tested on a CK6140 horizontal lathe manufactured by Chongqing Honggang CNC Machine Tool Co., Ltd. The experimental standard was: each set of inserts continuously fed 220 mm at 105 m / min until the feed distance was L = 2200 mm, and the wear on the flank face was measured.
[0053] The test results are as follows:
[0054] The coated cutting tool of the present invention has a coating adhesion of 108N, a nano-hardness of 33.43GPa, a cutting force of 73N, and a flank wear of 0.12mm. It has high strength, high toughness, and high adhesion, and its cutting life is much higher than that of traditional AlTiN coated cutting tools.
[0055] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention is limited to these examples; within the framework of the invention, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of the different aspects of the invention as described above, which are not provided in detail for the sake of brevity.
[0056] This invention is intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this invention should be included within the scope of protection of this invention.
Claims
1. A method for preparing a composite multilayer TiAlN / AlTiN / ZrN coated cutting tool, characterized in that, The specific preparation steps are as follows: (1) Place the substrate material in the vacuum coating equipment and adjust the vacuum level of the equipment to 8×10. -5 mbar, heated for 1 hour, raising the temperature to 460-480℃; (2) A first material layer is deposited on the substrate material using PVD process. The first material layer is a TiAlN layer. (3) A second material layer is deposited on the side of the first material layer away from the substrate material using PVD process. The second material layer is an AlTiN layer. (4) A third material layer is deposited on the side of the second material layer away from the substrate material using PVD process. The third material layer is a ZrN layer. (5) A fourth material layer is deposited on the side of the third material layer away from the substrate material using PVD process. The fourth material layer is an AlTiN layer. (6) A fifth material layer is deposited on the side of the fourth material layer away from the substrate material using PVD process. The fifth material layer is a ZrN layer. (7) A sixth material layer is deposited on the side of the fifth material layer away from the substrate material using PVD process. The sixth material layer is an AlTiN layer. (8) A seventh material layer is deposited on the side of the sixth material layer away from the substrate material using PVD process. The seventh material layer is a ZrN layer. The TiAlN layer described in step (2) is prepared using a TiAl target, wherein the molar ratio of Ti to Al in the TiAl target is 50 / 50. The AlTiN layer described in step (3) is prepared using TiAl and Al targets, wherein the molar ratio of Ti to Al in the TiAl target is 50 / 50. The method of depositing AlTiN layer using PVD process in steps (5) and (7) is the same as in step (3); the method of depositing ZrN layer using PVD process in steps (6) and (8) is the same as in step (4).
2. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, The matrix material mentioned in step (1) is cemented carbide.
3. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, In step (2), the first material layer includes multiple stacked bonding layers. The specific preparation steps are as follows: each bonding layer is deposited sequentially using PVD process. A single bonding layer is deposited. The TiAl target is placed in a nitrogen environment with a molecular pump frequency of 72%, a pressure of 2.5×10⁻¹mbar, an arc ignition current of 150A, a bias voltage of a preset voltage, and a temperature of 480℃ for a preset time. The N2 flow rate is 1200sccm. The bonding layer closer to the second material layer requires a larger bias voltage during film deposition.
4. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 3, characterized in that, The first bonding layer is deposited on the substrate material using PVD process, with a required bias voltage of 40V and a processing time of 40±2min; the second bonding layer is deposited on the substrate material, with a required bias voltage of 80V and a processing time of 2min; the third bonding layer is deposited on the substrate material, with a required bias voltage of 120V and a processing time of 30±2min.
5. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, The method for depositing the second material layer in step (3) is as follows: TiAl target and Al target are respectively placed in a nitrogen environment with a molecular pump frequency of 72%, a pressure of 2.5 × 10⁻¹ mbar, an arc current of 150A, a bias voltage of 80V, and a temperature of 480℃ for 2 minutes to obtain the second material layer on the substrate material. The N2 flow rate is 1200 sccm.
6. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, The method for depositing the third material layer in step (4) is as follows: placing the Zr target at a molecular pump frequency of 72% and a pressure of 2.5 × 10⁻⁶. -1 The third material layer can be formed on the substrate material by treating it in a nitrogen environment with mbar, arc current of 150A, bias voltage of 120V, and temperature of 480℃ for 30 minutes, with an N2 flow rate of 1200 sccm.
7. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, The first material layer includes multiple bonding layers arranged in a stacked manner, namely a first bonding layer, a second bonding layer and a third bonding layer.
8. The method for preparing the composite multilayer TiAlN / AlTiN / ZrN coated cutting tool according to claim 1, characterized in that, The thickness of the first material layer is between 1.0 and 1.2 μm, and the thickness of the second material layer is between 0.8 and 1.0 μm.
9. A composite multilayer TiAlN / AlTiN / ZrN coated cutting tool, characterized in that, It is prepared according to any one of claims 1-8.
Citation Information
Patent Citations
A multi-structure heterogeneous coating, its preparation method and application
CN116411244B
Ti-Zr / ZrN nanometer multilayer coating cutter and preparation process thereof
CN102181835A
Coated cutting tool with multi-layer structure and preparation method
CN118291919A
KR20230102644A