Corrosion-resistant local amorphous ferronickel ultrathin nanosheet anode electrocatalyst as well as preparation method and application of corrosion-resistant local amorphous ferronickel ultrathin nanosheet anode electrocatalyst
By using corrosion-resistant local amorphous nickel-iron ultra-thin nanosheet anode electrocatalyst in seawater electrolysis, the problems of high energy consumption and poor corrosion resistance of catalysts in seawater electrolysis are solved, and low energy consumption and high efficiency catalytic effects are achieved, suitable for seawater electrolysis. large-scale application.
Patent Information
- Application Number
- CN202411008096.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art has problems of high energy consumption and poor corrosion resistance of catalysts in seawater electrolysis, especially in high concentration chloride ion environments, which limits the efficiency and large-scale application of electrocatalytic decomposition of water.
A corrosion-resistant local amorphous nickel-iron ultra-thin nanosheet anode electrocatalyst is used to conduct corrosion oxidation and S2-local etching through a foam nickel-iron matrix under normal temperature and pressure to form a catalyst with high activity and corrosion resistance.
Low energy consumption and high efficiency catalysis in seawater electrolysis are achieved. The catalyst exhibits low overpotential and high stability under alkaline conditions, and can generate a large amount of O2 and H2 at low applied voltages, significantly reducing the energy consumption of electrolyzed seawater.
Smart Images

Figure CN118957623A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalyst materials, and in particular relates to a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst and a preparation method and application thereof. Background Art
[0002] As a green, low-carbon and clean energy, hydrogen has high calorific value and high energy density (140MJ·kg -1 ) is the key to achieving net zero emissions and addressing global warming. Water / seawater electrolysis technology powered by renewable energy has good development potential in industrial hydrogen production. In the context of scarce freshwater resources, seawater electrolysis can be used as a long-term goal for the construction of a hydrogen economy. Among them, the anode reaction (oxygen evolution reaction, OER) of electrocatalytic water decomposition involves a slow multi-proton coupled electron transfer process with high energy requirements and thermodynamic barriers, which limits the large-scale application of electrocatalytic water / seawater decomposition hydrogen production technology. In addition, the complex seawater environment, especially the high concentration of chloride ions (Cl - ) will lead to electrode corrosion and other side reactions, further reducing the catalytic efficiency. Highly efficient and corrosion-resistant oxygen evolution electrocatalysts can effectively reduce the overpotential of the OER reaction, thereby significantly reducing the energy consumption of hydrogen production by electrolyzing seawater.
[0003] Currently, noble metal oxides (RuO2 or IrO2) are the OER catalysts with the best catalytic performance, but the scarcity and high price of noble metals limit their large-scale application. In recent years, transition metal (oxy)hydroxides have shown amazing potential in OER. Layered hydroxides are prone to accumulation and aggregation, which will inevitably limit the full exposure of active sites and affect catalytic performance. Disordered amorphous nanomaterials induce the formation of a large number of suspended bonds and defects, which are beneficial to the full exposure of active sites, improve electrocatalytic activity and corrosion resistance under seawater electrolysis. However, the disordered structure of the amorphous phase will hinder the transfer of carriers, severely limit the charge transfer kinetics, and cause a decrease in catalytic activity and corrosion resistance.
[0004] For example, the Chinese patent application with application number 202110178409.2 also discloses a nickel foam-supported sulfide electrocatalyst and its preparation method and application, but it adopts the traditional hydrothermal reaction method, uses a variety of nitrates for deposition, and requires the addition of urea to provide an alkaline environment. The preparation process is complicated, and the catalytic performance of the obtained catalyst is average. The corrosion resistance of the material itself is poor, so it is difficult to apply in practice, let alone in seawater electrolysis.
[0005] Therefore, adjusting the crystalline-amorphous phase structure of the catalytic material through a simple, efficient, and energy-saving preparation process is very necessary to balance the high activity and strong corrosion resistance under seawater conditions and realize large-scale hydrogen production by electrolysis of seawater. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a highly efficient, corrosion-resistant and low-cost locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst for seawater electrolysis, which can effectively reduce the overpotential of the OER reaction, and at the same time provides a simple, efficient and convenient preparation method of the catalyst.
[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0008] A corrosion-resistant locally amorphous nickel-iron ultra-thin nanosheet anode electrocatalyst is used. The foamed nickel-iron matrix is corroded and oxidized by FeCl3 and H2O2 at room temperature and pressure to form crystalline nickel-iron hydroxide ultra-thin nanosheets. 2- The supporting points of the nickel-iron hydroxide lattice structure are locally etched to obtain the final product catalyst.
[0009] A method for preparing a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst comprises the following preparation steps:
[0010] (1) The nickel-iron foam was ultrasonically cleaned with hydrochloric acid solution, anhydrous ethanol and deionized water for 30 minutes to remove impurities on the surface;
[0011] (2) placing the cleaned nickel-iron foam in step (1) in a FeCl3 solution, and adding a H2O2 solution dropwise thereto, and obtaining a crystalline electrocatalyst having ultrathin nanosheets after the reaction is completed;
[0012] (3) placing the crystalline electrocatalyst obtained in step (2) in a Na2S solution and maintaining it in a water bath at 60°C for 4 hours.
[0013] After the reaction is completed, a locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst is obtained.
[0014] Furthermore, the nickel iron foam in step (1) has a length of 30 mm, a width of 5 mm, a thickness of 1.6 mm, and a porosity of 96%.
[0015] Furthermore, the ultrasonic cleaning of step (1) for 30 minutes is the total cleaning time, that is, ultrasonic cleaning with hydrochloric acid solution for 10 minutes, ultrasonic cleaning with anhydrous ethanol for 10 minutes, and finally cleaning with deionized water for 10 minutes.
[0016] Furthermore, the concentration of the hydrochloric acid solution in step (1) is 1M.
[0017] Furthermore, the concentration of the FeCl3 solution in step (2) is 0.05M and the amount used is 20mL.
[0018] Furthermore, in step (2), the mass concentration of the H2O2 solution is 30 wt%, the dropping time is 30 min, and the dropping speed is 0.05 mL / min.
[0019] Furthermore, the concentration of the Na2S solution in step (2) is 0.5 M and the amount used is 30 mL.
[0020] The invention discloses an application of a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst, wherein the catalyst is applied to seawater electrolysis.
[0021] The catalyst of the present invention is obtained by rapidly preparing nickel-iron-based ultra-thin nanosheets on the surface of a nickel-iron foam substrate by in-situ etching treatment based on the Fenton reaction principle, and then subjecting the nanosheets to local amorphization treatment. In step (1) of the preparation method, FeCl3 and H2O2 are used as oxidants to corrode and oxidize the nickel-iron foam substrate, thereby promoting the formation of Fe on the surface of the nickel-iron foam. 2+ / Ni 2+ The H2O2 added dropwise and Fe 2+ Fenton reaction further generates Fe 3+ , which accelerates the surface corrosion process and increases the local pH value on the surface of nickel-iron foam. 3+ with Ni 2+ In-situ deposition on the surface of nickel-iron foam. During the deposition process, the O2 generated by the decomposition of H2O2 increases the interlayer spacing of nickel-iron hydroxide during violent movement and escape, forming ultra-thin crystalline nickel-iron hydroxide nanosheets. In the process of local amorphization, the destructive S 2- The support points of the nickel-iron hydroxide lattice structure are locally etched to obtain a locally amorphous nickel-iron-based electrocatalyst.
[0022] Beneficial Effects
[0023] (1) The preparation method of the present invention is fast, simple, energy-efficient, and has a short catalyst growth cycle. It can prepare ultrathin nanosheets with local amorphization and large interlayer spacing without high temperature, high pressure, or other preparation conditions. The catalyst exhibits satisfactory OER catalytic activity in alkaline fresh water and seawater. -2 The current density has a low overpotential (η 淡水 =245mV,η 海水 =252mV), Tafel slope (55.8mV·dec -1) and high long-term stability (can run continuously and stably for more than 100 hours under alkaline natural seawater conditions). Therefore, the local amorphous nickel-iron-based electrocatalyst obtained by the energy-efficient method of the present invention has strong corrosion resistance in a seawater environment and can effectively reduce the overpotential and energy consumption of the OER reaction;
[0024] (2) The present invention obtains a partially amorphous nickel-iron-based electrocatalyst by S etching, which has low energy consumption and preparation cost, and exhibits a low reaction overpotential, so that the electrolysis of seawater can be carried out under a low applied voltage, thereby producing more O2 and H2; in a two-electrode system, it reaches 500mA·cm -2 The external voltage required at high current density is only 1.83V;
[0025] (3) The catalyst of the present invention has an ultrathin nanosheet microstructure. Experimental and DFT calculation results show that the catalyst has a large electrochemical specific surface area, which is conducive to full contact and rapid diffusion between the active sites and the electrolyte;
[0026] (4) The catalyst of the present invention uses S etching to adjust the electronic configuration and accelerate surface reconstruction. The etching time is appropriate, so that the local amorphous region with abundant unsaturated active sites enhances the lattice oxygen activity, reduces the desorption energy of O2, and accelerates the OER process through the LOM mechanism. In addition, the preferentially adsorbed OH - and surface reconstructed SO4 2- Together they prevented Cl - The catalyst of the present invention exhibits excellent OER catalytic activity and strong corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 XRD patterns of electrocatalysts la-S-NiFe-LDH / NFF and NiFe-LDH / NFF;
[0028] Figure 2 The microscopic morphology of the electrocatalyst NiFe-LDH / NFF;
[0029] Figure 3 The microscopic morphology of the electrocatalyst la-S-NiFe-LDH / NFF;
[0030] Figure 4 The XPS total spectra of the electrocatalysts la-S-NiFe-LDH / NFF and NiFe-LDH / NFF, wherein (a) is the XPS total spectrum of the electrocatalyst, (b) is the Ni 2p high-resolution spectrum, (c) is the Fe 2p high-resolution spectrum, (d) is the S2p high-resolution spectrum, and (e) is the O1s high-resolution spectrum;
[0031] Figure 5 This is the microscopic morphology of the sample NiFe-OH / NFF of Comparative Example 1;
[0032] Figure 6 XRD patterns of comparative samples S-NiFe-LDH / NFF-1h, S-NiFe-LDH / NFF-2h, La-S-NiFe-LDH / NFF and S-NiFe-LDH / NFF-12h;
[0033] Figure 7 The microscopic morphology of comparative samples S-NiFe-LDH / NFF-1h, S-NiFe-LDH / NFF-8h and S-NiFe-LDH / NFF-12h at different magnifications, where (ab) are S-NiFe-LDH / NFF-1h, (cd) S-NiFe-LDH / NFF-8h, (ef) S-NiFe-LDH / NFF-12h;
[0034] Figure 8 It is the LSV curve diagram of Example 1 and Comparative Examples 2-6 samples;
[0035] Fig. 9 LSV curves of samples la-S-NiFe-LDH / NFF, NiFe-LDH / NFF, NiFe-OH / NFF, IrO2 and NFF;
[0036] Fig.10 The Tafel curves of samples la-S-NiFe-LDH / NFF, NiFe-LDH / NFF, NiFe-OH / NFF, IrO2 and NFF;
[0037] Fig.11 EIS spectra of samples la-S-NiFe-LDH / NFF, NiFe-LDH / NFF, NiFe-OH / NFF, IrO2 and NFF:
[0038] Fig.12 Cdl diagrams of samples la-S-NiFe-LDH / NFF, NiFe-LDH / NFF, NiFe-OH / NFF, IrO2 and NFF;
[0039] Fig.13 LSV curves of sample la-S-NiFe-LDH / NFF in different electrolytes;
[0040] Fig.14 Corrosion polarization curves of samples la-S-NiFe-LDH / NFF, NiFe-LDH / NFF, NiFe-OH / NFF and NFF;
[0041] Fig.15 The stability diagram of sample la-S-NiFe-LDH / NFF in 1M KOH and 1M KOH+natural seawater;
[0042] Fig.16 Ni-3d band DOS diagram of samples la-S-NiFe-LDH / NFF and NiFe-LDH / NFF;
[0043] Fig.17 The O-2p band DOS diagram of samples la-S-NiFe-LDH / NFF and NiFe-LDH / NFF;
[0044] Fig.18 Gibbs free energy step diagram of samples la-S-NiFe-LDH / NFF and NiFe-LDH / NFF;
[0045] Fig.19 The OH of samples la-S-NiFe-LDH / NFF and NiFe-LDH / NFF - Adsorption free energy diagram. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.
[0047] Example 1
[0048] A method for preparing a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst comprises the following preparation steps:
[0049] (1) A nickel-iron foam with a length of 30 mm, a width of 5 mm, a thickness of 1.6 mm, and a porosity of 96% was ultrasonically cleaned with 1 M HCl solution, anhydrous ethanol, and deionized water for 10 minutes respectively, for a total of 30 minutes, to remove surface impurities;
[0050] (2) The cleaned nickel-iron foam was placed in 20 mL of a 0.05 M FeCl3 uniform solution, and a 30 wt % H2O2 solution was added thereto at a rate of 0.05 mL / min for 30 min at room temperature. After the addition was completed, a crystalline NiFe-LDH / NFF electrocatalyst with ultrathin nanosheets was obtained;
[0051] (3) NiFe-LDH / NFF was then placed in 30 mL of 0.5 M Na2S solution and kept in a 60°C water bath for 4 h. After the reaction was completed, a partially amorphous S-modified nickel-iron-based electrocatalyst la-S-NiFe-LDH / NFF was obtained, which was the final product catalyst.
[0052] The crystal structures of la-S-NiFe-LDH / NFF and NiFe-LDH / NFF electrocatalysts were obtained by X-ray diffraction, such as Figure 1 As shown in Figure 3, the crystallinity of NiFe-LDH is significantly reduced after S local amorphization treatment.
[0053] The microstructures of the la-S-NiFe-LDH / NFF and NiFe-LDH / NFF electrocatalysts were obtained using scanning electron microscopy. Figure 2 As shown in the figure, a large number of nanosheets in the NiFe-LDH / NFF electrocatalyst are stacked to form a grid structure, which is stacked and grown on the surface of the nickel-iron foam skeleton. After S-modified local amorphization treatment, the support points around the la-S-NiFe-LDH / NFF electrocatalyst nanosheets are slightly etched and shrink in different directions, such as Figure 3 shown.
[0054] The XPS images of la-S-NiFe-LDH / NFF and NiFe-LDH / NFF electrocatalysts were obtained by X-ray photoelectron spectroscopy, as shown in Figure 4 As shown in the figure, after S local amorphization treatment, the electron density around the metal center is reduced, the valence state of Ni / Fe is increased, and the local amorphous nanostructure formed by S regulation has abundant unsaturated defects.
[0055] Comparative Example 1
[0056] A method for preparing an anode electrocatalyst comprises the following preparation steps:
[0057] (1) A nickel-iron foam with a length of 30 mm, a width of 5 mm, a thickness of 1.6 mm, and a porosity of 96% was ultrasonically cleaned with 1 M HCl solution, anhydrous ethanol, and deionized water for 10 minutes respectively, for a total of 30 minutes, to remove surface impurities;
[0058] (2) The cleaned nickel-iron foam was placed in 20 mL of 0.05 M FeCl3 uniform solution and kept at room temperature for 30 min without adding H2O2 solution. After the reaction was completed, crystalline NiFe-OH / NFF was obtained.
[0059] The microscopic morphology of the samples was obtained using a scanning electron microscope. Figure 5 As shown, irregular floccules are dispersed on the surface of nickel-iron foam, rather than ultra-thin nanosheet structures. It can be seen that the use of hydrogen peroxide in the present invention not only accelerates the oxidation, but also plays an important role in the formation of the special morphology of the catalyst of the present invention.
[0060] Comparative Examples 2-6
[0061] A method for preparing an anode electrocatalyst comprises the following preparation steps:
[0062] (1) A nickel-iron foam with a length of 30 mm, a width of 5 mm, a thickness of 1.6 mm, and a porosity of 96% was ultrasonically cleaned with 1 M HCl solution, anhydrous ethanol, and deionized water for 10 minutes respectively, for a total of 30 minutes, to remove surface impurities;
[0063] (2) The cleaned nickel-iron foam was placed in 20 mL of a 0.05 M FeCl3 uniform solution, and a 30 wt % H2O2 solution was added thereto at a rate of 0.05 mL / min for 30 min at room temperature. After the addition was completed, a crystalline NiFe-LDH / NFF electrocatalyst with ultrathin nanosheets was obtained;
[0064] (3) Then NiFe-LDH / NFF was placed in 30 mL of 0.5 M Na2S solution and kept in a water bath at 60°C for 1 h, 2 h, 6 h, 8 h, and 12 h, respectively, to obtain electrocatalysts after the reaction. The obtained catalysts were referred to as S-NiFe-LDH / NFF-1h, S-NiFe-LDH / NFF-2h, S-NiFe-LDH / NFF-6h, S-NiFe-LDH / NFF-8h, and S-NiFe-LDH / NFF-12h, respectively.
[0065] The experimental process of Comparative Examples 2-6 is the same as the preparation process of the electrocatalyst la-S-NiFe-LDH / NFF in Example 1, with the difference being that the immersion time is changed during the 0.5M Na2S solution water bath treatment, and the immersion times are 1h, 2h, 6h, 8h, and 12h under the same conditions, respectively.
[0066] The crystal structure of the corresponding sample was obtained by X-ray diffraction, such as Figure 6 As shown in Figure 2, as the reaction time increases, the crystallinity of the sample gradually decreases and gradually transforms into an amorphous state. The microscopic morphology of the sample obtained by scanning electron microscopy is shown in Figure 2. Figure 7 As shown in Figure 2, after a long period of water bath reaction, the ultra-thin nanosheets gradually transformed into thicker particle sheets, and the network structure eventually collapsed. Figure 8 As shown, the LSV curve of the sample shows that the sample obtained when the water bath reaction time is 4h (Example 1 of the present invention) has the best electrocatalytic performance.
[0067] Performance Testing
[0068] The electrochemical performance was carried out in a three-electrode system of a CHI 760E workstation, where the prepared sample was used as the working electrode (the test geometry area was 0.5 × 0.4 cm 2), Hg / HgO and graphite rod were used as reference electrode and counter electrode, respectively, and the electrolytes were 1M KOH, 1M KOH+0.5M NaCl, and 1M KOH+natural seawater solution.
[0069] The performance of different types of catalysts were compared. The test samples were: la-S-NiFe-LDH / NFF (Example 1), NiFe-LDH / NFF, NiFe-OH / NFF (Comparative Example 1), IrO2 and NFF (nickel iron foam).
[0070] In 1M KOH electrolyte, the LSV curve of the electrocatalyst of Example 1 of the present invention is as follows: Fig. 9 As shown in Figure 2, the S-modified locally amorphous NiFe-based catalyst la-S-NiFe-LDH / NFF exhibited the best electrocatalytic performance at a current density of 100 mA cm -2 The required overpotential is 245mV.
[0071] The Tafel curves of different catalysts are as follows: Fig.10 As shown, the Tafel slope of la-S-NiFe-LDH / NFF is 55.8mVdec -1 .
[0072] EIS spectra of different catalysts are shown in Figure 2. Fig.11 As shown, the la-S-NiFe-LDH / NFF electrocatalyst exhibits the smallest electrochemical impedance.
[0073] The double layer capacitance of different catalysts is Fig.12 As shown, the la-S-NiFe-LDH / NFF electrocatalyst has the largest Cdl value, indicating that it has the largest electrochemical specific surface area.
[0074] In 1M KOH+ natural sea electrolyte, the LSV curve is as follows Fig.13 As shown in Figure 2, la-S-NiFe-LDH / NFF exhibits excellent electrocatalytic performance at 100 mA cm -2 When the overpotential is 252mV, the corrosion polarization curve is as follows Fig.14 As shown in Figure 2, the la-S-NiFe-LDH / NFF electrocatalyst exhibits the best corrosion resistance. Fig.15 As shown, after 100 hours of continuous operation, the activity of la-S-NiFe-LDH / NFF did not decrease significantly.
[0075] The electronic structure of the catalysts was studied by first principles using la-S-NiFe-LDH / NFF and NiFe-LDH / NFF. The Gibbs free energy was calculated using Formula: G = Eads + ZPE-TS. Fig.16 and 17 As shown in Figure 2, the la-S-NiFe-LDH / NFF electrocatalyst significantly enhances the lattice oxygen activity. The Gibbs free energy step diagram of the sample is shown in Figure 2. Fig.18 As shown in Figure 2, la-S-NiFe-LDH / NFF effectively reduces the desorption energy of O2, which is beneficial to the rapid release of O2. Fig.19 It is shown that compared with NiFe-LDH / NFF, OH - It is more conducive to adsorption on the surface of la-S-NiFe-LDH / NFF. According to Pearson principle, OH - The preferential adsorption of Cl - The proximity and erosion of la-S-NiFe-LDH / NFF improves the seawater electrolytic corrosion resistance.
[0076] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst, It is characterized in that Using nickel-iron foam as the matrix, at room temperature and pressure, FeCl 3 and H 2 O 2 The foamed nickel-iron matrix is corroded and oxidized to form ultra-thin nanosheets of crystalline nickel-iron hydroxide, and then the destructive S 2- The supporting points of the nickel-iron hydroxide lattice structure are locally etched to obtain the final product catalyst.
2. A method for preparing a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst, It is characterized in that The method comprises the following preparation steps: (1) The nickel-iron foam was ultrasonically cleaned for 30 minutes using hydrochloric acid solution, anhydrous ethanol and deionized water in sequence to remove impurities on the surface; (2) Place the cleaned nickel-iron foam in FeCl 3 solution, and H 2 O 2 solution, and after the reaction is completed, a crystalline electrocatalyst having ultrathin nanosheets is obtained; (3) placing the crystalline electrocatalyst obtained in step (2) in a Na 2 S solution and kept in a 60°C water bath for 4 h. After the reaction, a locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst was obtained.
3. The method for preparing the corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst according to claim 2, It is characterized in that Step (1) The nickel iron foam has a length of 30 mm, a width of 5 mm, a thickness of 1.6 mm, and a porosity of 96%.
4. The method for preparing the corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst according to claim 2, It is characterized in that The concentration of the hydrochloric acid solution in step (1) is 1M.
5. The method for preparing the corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst according to claim 2, It is characterized in that Step (2) FeCl 3 The concentration of the solution is 0.05M and the amount used is 20mL.
6. The method for preparing the corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst according to claim 2, It is characterized in that Step (2) H 2 O 2 The mass concentration of the solution was 30 wt %, the dropping time was 30 min, and the dropping speed was 0.05 mL / min.
7. The method for preparing the corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst according to claim 2, It is characterized in that Na 2 The concentration of S solution is 0.5M and the amount used is 30mL.
8. Application of a corrosion-resistant locally amorphous nickel-iron ultrathin nanosheet anode electrocatalyst, It is characterized in that The catalyst is applied to seawater electrolysis.