Iridium-based supported catalyst as well as preparation method and application thereof

By forming a supported catalyst with an iridium oxide shell layer on the surface of the titanium dioxide support, the problem of slow oxygen precipitation reaction kinetics of the iridium-based catalyst in PEM electrolytic water is solved, the conductivity and electrolytic efficiency of the catalyst are improved, and the iridium loading is achieved and the balance of catalytic properties.

CN118957635AActive Publication Date: 2024-11-15TSINGHUA UNIVERSITY

Patent Information

Application Number
CN202411138760.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing iridium-based catalysts are slow in the proton exchange membrane electrolyzed water due to the slow kinetics of oxygen precipitation reaction (OER) and require high potential driving, which leads to a problem of reducing the energy conversion efficiency and reducing the iridium load while maintaining high catalytic performance.

Method used

IrOx@TiO2 catalyst is formed by in situ reaction on the surface of the titanium dioxide support, and the oxide of iridium is uniformly coated with nano-thickness to form a continuous supported catalyst, which improves conductivity and reduces the iridium load.

Benefits of technology

The balance between high catalytic performance and low iridium load in PEM electrolytic water is achieved, the conductivity and oxygen precipitation performance of the catalyst are improved, and the efficiency of electrolytic water is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957635A_ABST
    Figure CN118957635A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and provides an iridium-based supported catalyst, a preparation method of the iridium-based supported catalyst, a proton exchange membrane electrolysis water membrane electrode and application of the iridium-based catalyst. The preparation method comprises the following steps: taking titanium dioxide as a carrier, carrying out hydrolysis reaction on an iridium precursor and an alkaline substance, and carrying out oxidation reaction on a hydrolysis reaction product and hydrogen peroxide to obtain a precursor of the iridium-based supported catalyst; a precursor of the iridium-based supported catalyst is subjected to calcination treatment in the presence of oxygen, the iridium-based supported catalyst IrOx-coated TiO2 is prepared, x is equal to 1-2, and IrOx serves as a shell layer to be coated on the surface of a TiO2 core body. The iridium oxide of the catalyst uniformly forms a shell structure on the surface of titanium dioxide, the catalytic performance of the catalyst is effectively improved, the iridium loading amount is effectively reduced, and the iridium-based catalyst IrOx-coated TiO2 has excellent electrolysis performance in PEM electrolyzed water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and specifically relates to an iridium-based supported catalyst and a preparation method thereof, as well as applications of a proton exchange membrane water electrolysis membrane electrode and an iridium-based catalyst. Background Art

[0002] Hydrogen energy is an indispensable energy carrier due to its high energy density and zero carbon emissions. Currently, PEM (Proton Exchange Membrane (PEM)) water electrolysis and alkaline water electrolysis coupled with photovoltaic or wind power are very promising ways to produce green hydrogen. PEM water electrolysis has attracted much attention due to its high current density, high energy conversion efficiency, high hydrogen purity and high responsiveness. However, in the PEM water electrolysis process, the anode requires a high potential to drive the reaction due to the slow reaction kinetics of the oxygen evolution reaction (OER), which reduces the energy conversion efficiency of the PEM electrolyzer. Under the harsh working conditions of the anode (high potential, pure oxygen environment, high acidity), iridium catalysts have become the mainstream commercial catalysts for PEM water electrolysis due to their excellent stability and catalytic activity.

[0003] At present, the power density of iridium per unit mass cannot meet the actual demand. Therefore, reducing the iridium loading in the catalyst layer and improving the utilization rate of iridium are crucial for the large-scale application of PEMWE (Proton Exchange Membrane Water Electrolysis). However, at present, the prepared supported catalysts are all iridium-based catalysts distributed on the carrier, which requires a higher loading to improve its conductivity and thus improve the catalytic performance, which is contrary to the original intention of reducing the iridium loading. The conductivity of low iridium catalysts is poor, and there is a high ohmic loss in PEMWE. Summary of the invention

[0004] The present invention aims to solve the technical problem of reducing iridium loading and maintaining high catalytic performance at least to a certain extent. To this end, an object of the present invention is to provide an iridium-based supported catalyst and a preparation method thereof, as well as a proton exchange membrane water electrolysis membrane electrode and an application of the iridium-based catalyst. The oxide of the catalyst iridium uniformly forms a shell structure on the surface of titanium dioxide, effectively maintaining high catalytic performance and reducing iridium loading.

[0005] The first aspect of the present application provides a method for preparing an iridium-based supported catalyst. According to an embodiment of the present invention, the method comprises: using titanium dioxide as a carrier, hydrolyzing an iridium precursor with an alkaline substance, and then oxidizing the hydrolysis reaction product with hydrogen peroxide to obtain a precursor of the iridium-based supported catalyst; calcining the precursor of the iridium-based supported catalyst in an atmosphere in the presence of oxygen to prepare an iridium-based supported catalyst IrO x@TiO2, where x = 1 to 2, IrO x As a shell layer coated on the surface of TiO2 core.

[0006] The present invention forms a coating layer of iridium oxide on the surface of a titanium dioxide carrier by in-situ reaction through alkaline hydrolysis, oxidation and reoxidation. The iridium oxide is uniformly coated on the titanium dioxide surface with a nanometer thickness to form a fully covered continuous supported catalyst, which is conducive to forming a good electronic conductive network and improving the conductivity of the catalyst. At the same time, the supported catalyst formed by the in-situ reaction of the present invention has a high catalytic performance while reducing the iridium loading, which is conducive to balancing the iridium content and catalytic performance of the supported catalyst.

[0007] According to an embodiment of the present invention, the preparation method of the iridium-based supported catalyst may further include at least one of the following additional technical features:

[0008] In some embodiments, the raw material satisfies at least one of the following (1) to (3):

[0009] (1) The iridium precursor includes at least one of IrCl3, Na3IrCl6, Na2IrCl6 and H2IrCl6;

[0010] (2) the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate and lithium carbonate;

[0011] (3) The morphology of titanium dioxide includes at least one of titanium dioxide nanoparticles, titanium dioxide nanowires and titanium dioxide nanorods.

[0012] In some embodiments, in the step of hydrolysis reaction: the parameter pH value is controlled to be 9-13.

[0013] In some embodiments, in the calcination step, the control parameters meet the following conditions: the calcination temperature is 250° C. to 450° C.; and / or the calcination time is 0.5 h to 2 h.

[0014] In some embodiments, the molar mass ratio of iridium atoms to hydrogen peroxide in the iridium precursor is 1:20 to 1:1000; and / or the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is 1:1 to 1:10.

[0015] In some embodiments, the hydrolysis reaction and the oxidation reaction comprise the steps of:

[0016] preparing an iridium precursor in aqueous solution;

[0017] adding titanium dioxide into the aqueous solution to prepare a dispersion;

[0018] adding an alkaline substance to the dispersion to carry out a hydrolysis reaction;

[0019] Hydrogen peroxide is added to the hydrolysis reaction system to carry out an oxidation reaction.

[0020] The second aspect of the present application provides an iridium-based supported catalyst. According to an embodiment of the present invention, the iridium-based supported catalyst comprises a core body and a shell layer coated outside the core body; the core body comprises TiO2, and the shell layer comprises IrO x , where x=1~2.

[0021] The iridium-based supported catalyst IrO x @TiO2 is a core-shell structure in which iridium oxide is uniformly coated on the surface of titanium dioxide, and the value of x is 1 to 2, that is, the iridium oxide can be a multivalent iridium oxide. The catalyst can effectively reduce the iridium loading and has high conductivity and catalytic performance.

[0022] In some embodiments, the iridium-based supported catalyst is prepared by the above-mentioned preparation method, IrO x The mass percentage is 20% to 75%.

[0023] The third aspect of the present application provides a proton exchange membrane water electrolysis membrane electrode, comprising the iridium-based supported catalyst obtained by the above-mentioned preparation method, or comprising the above-mentioned iridium-based supported catalyst.

[0024] The iridium-based catalyst IrO provided in this application x @TiO2, the iridium oxide shell fully covers the titanium dioxide surface, with a thickness of only a few nanometers, which effectively reduces the iridium loading and increases its catalytic performance. The core-shell catalyst has excellent oxygen evolution performance and excellent electrolysis performance in PEM water electrolysis.

[0025] In a fourth aspect, the present application provides an application of an iridium-based supported catalyst in a water electrolysis reaction, wherein the iridium-based supported catalyst is the iridium-based supported catalyst obtained by the above-mentioned preparation method, or is the above-mentioned iridium-based supported catalyst.

[0026] The iridium-based catalyst IrO provided in this application x @TiO2 has excellent electrolytic performance in PEM electrolysis of water.

[0027] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0029] Figure 1 The 40% IrO provided in Example 1 of the present application x @Element mapping of TiO2-NP catalyst.

[0030] Figure 2 The 40% IrO provided in Example 1 of the present application x @Element mapping of TiO2-NR catalyst.

[0031] Figure 3 The 20% IrO provided in Example 2 of this application x @Element mapping of TiO2-NW catalyst.

[0032] Figure 4 The 40% IrO provided in Example 1 of the present application x @Element content test results of TiO2-NP catalyst.

[0033] Figure 5 The 40% IrO provided in Example 1 of the present application x @Element content test results of TiO2-NR catalyst.

[0034] Figure 6 The 20% IrO provided in Example 2 of this application x @Element content test results of TiO2-NW catalyst.

[0035] Figure 7 This is a graph showing the OER performance test results of the catalyst provided in the examples of the present application.

[0036] Figure 8 Schematic diagram of the electrolysis water performance test structure in the performance test of this application.

[0037] Fig. 9 This is a graph showing the water electrolysis performance test results of the catalyst provided in the examples of the present application. DETAILED DESCRIPTION

[0038] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0039] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.

[0040] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0041] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.

[0042] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.

[0043] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.

[0044] The first aspect of the present application provides a method for preparing an iridium-based supported catalyst, comprising: using titanium dioxide as a carrier, hydrolyzing an iridium precursor with an alkaline substance, and then oxidizing the hydrolysis reaction product with the hydrogen peroxide to obtain a precursor of the iridium-based supported catalyst; calcining the precursor of the iridium-based supported catalyst in an atmosphere in the presence of oxygen to prepare an iridium-based supported catalyst IrO x @TiO2, where x = 1 to 2, IrO x As a shell layer coated on the surface of TiO2 core.

[0045] At present, there are usually two methods to reduce the iridium loading: using iridium-based nanowire catalysts and using carriers to load iridium to prepare catalysts. For iridium-based nanowire catalysts, the preparation process is relatively complicated and difficult to mass-produce. Using carriers to prepare iridium-based catalysts can improve the dispersibility of iridium metal and increase the number of reaction sites. Titanium dioxide is a carrier with a wide range of sources and excellent stability. It has been widely reported in academia and industry. However, titanium dioxide is a nearly insulating carrier that requires a high iridium content to improve its conductivity. It is difficult to achieve a high conductivity while reducing the iridium content. In addition, the current supported catalysts are almost all iridium-based nanoparticles dispersed on a carrier. PEMWE electrolysis is a process involving electrons, protons, water and oxygen. It is very important to provide a good conductive network for the OER reaction. Due to the discontinuity of iridium dioxide, the current dispersed supported catalysts cannot build an electron-conducting conductive network, which seriously affects the efficiency of water electrolysis and the service life of the catalyst.

[0046] The present invention prepares an iridium oxide coating layer in situ on the surface of a titanium dioxide carrier through alkaline hydrolysis, oxidation and high-temperature calcination processes. The iridium oxide is uniformly coated on the titanium dioxide surface with a nanometer thickness to form a fully covered continuous supported catalyst, which is conducive to forming a good electronic conductive network and improving the conductivity of the catalyst. At the same time, the supported catalyst formed by the in-situ reaction of the present invention has a high catalytic performance while reducing the iridium loading, which is conducive to balancing the iridium content and catalytic performance of the supported catalyst.

[0047] In the present application, an iridium precursor is subjected to an alkaline hydrolysis reaction to prepare iridium hydroxide; the iridium hydroxide is then oxidized to iridium oxide through the oxidation action of hydrogen peroxide; finally, through a calcination treatment, part or all of the low-valent iridium oxide is further oxidized to become a higher-valent iridium oxide, which is conducive to the uniform distribution of the iridium oxide on the surface of titanium dioxide, effectively achieving a balance between catalytic performance and loading.

[0048] In some embodiments, the raw material satisfies at least one of the following (1) to (3):

[0049] (1) The iridium precursor includes at least one of IrCl3, Na3IrCl6, Na2IrCl6 and H2IrCl6;

[0050] (2) the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate and lithium carbonate;

[0051] (3) The morphology of titanium dioxide includes at least one of titanium dioxide nanoparticles, titanium dioxide nanowires and titanium dioxide nanorods.

[0052] In the embodiment of the present application, the precursor of iridium includes at least one of IrCl3, Na3IrCl6, Na2IrCl6 and H2IrCl6, which can be dissolved in an aqueous solvent and fully contact with the added alkaline substance to undergo a hydrolysis reaction, thereby helping to improve the reaction efficiency.

[0053] Furthermore, the precursor of iridium is at least one of IrCl3 and H2IrCl6.

[0054] In the embodiment of the present application, the alkaline substance is used to provide an alkaline environment to promote the hydrolysis reaction of the iridium precursor. The alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate and lithium carbonate, which is conducive to pH control and has low cost.

[0055] Furthermore, the alkaline substance includes at least one of sodium hydroxide and potassium hydroxide.

[0056] In the embodiment of the present application, the morphology of titanium dioxide includes at least one of titanium dioxide nanoparticles, titanium dioxide nanowires and titanium dioxide nanorods.

[0057] Furthermore, the morphology of titanium dioxide is titanium dioxide nanoparticles.

[0058] In some embodiments, the raw materials meet the following requirements: the iridium precursor includes at least one of IrCl3, Na3IrCl6, Na2IrCl6 and H2IrCl6; the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate and lithium carbonate; the morphology of titanium dioxide includes at least one of titanium dioxide nanoparticles, titanium dioxide nanowires and titanium dioxide nanorods.

[0059] In some embodiments, in the step of hydrolysis reaction: the parameter pH value is controlled to be 9-13.

[0060] In the embodiment of the present application, the pH value of the alkaline hydrolysis reaction is controlled to be 9 to 13, which is conducive to promoting the hydrolysis reaction of the iridium precursor, and within a reasonable range, the higher the pH value, the more conducive to the occurrence of the hydrolysis reaction, and the later oxidation to form a higher purity iridium oxide. If the pH value is too low, it is not conducive to the occurrence of the hydrolysis reaction, resulting in the inability to form a higher purity iridium oxide during the later oxidation and reoxidation process, thereby reducing the load of the iridium oxide. If the pH value is too high, it is a strong alkaline environment, which is conducive to the occurrence of the hydrolysis reaction, but has high requirements for the reaction operation and equipment.

[0061] In a specific example, in the step of hydrolysis reaction: the parameter pH value is controlled to be 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5 or 13, etc.

[0062] Furthermore, in the step of hydrolysis reaction: the parameter pH value is controlled to be 9-10.

[0063] In some embodiments, in the calcination step, the control parameters meet the following conditions: the calcination temperature is 250° C. to 450° C.; and / or the calcination time is 0.5 h to 2 h.

[0064] In the embodiment of the present application, the precursor of the iridium-based supported catalyst is calcined in an atmosphere of oxygen to further oxidize the low-valent iridium oxide to generate a higher-valent iridium oxide. By properly setting the calcination temperature, the low-valent iridium is oxidized to a higher-valent iridium to form a higher-valent iridium oxide, i.e., the iridium-based supported catalyst IrO x In @TiO2, the value of x becomes larger, while avoiding the generation of other impurities, forming an oxide shell structure of iridium with higher purity. In the specific example, the calcination temperature is 250℃, 280℃, 300℃, 320℃, 340℃, 350℃, 360℃, 380℃, 400℃ and 450℃, etc.; the calcination time is 0.5h, 1h, 1.5h, 2.0h, etc.

[0065] In the embodiments of the present application, the calcination temperature is 250° C. to 450° C., which is beneficial to improving the durability of the catalyst and at the same time helps to avoid increased crystallinity and decreased activity.

[0066] Furthermore, in the calcination step, the control parameters meet the following conditions: the calcination temperature is 300°C to 400°C.

[0067] In some embodiments, the molar mass ratio of iridium atoms to hydrogen peroxide in the iridium precursor is 1:20 to 1:1000; and / or the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is 1:1 to 1:10.

[0068] In an embodiment of the present application, the molar mass ratio of iridium atoms to hydrogen peroxide in the iridium precursor is set to 1:20 to 1:1000. In a specific example, the molar mass ratio of iridium atoms to hydrogen peroxide in the iridium precursor is set to 1:20, 1:50, 1:100, 1:200, 1:250, 1:300, 1:350, 1:400, 1:450, 1:500, 1:550, 1:600, 1:650, 1:700, 1:750, 1:800, 1:850, 1:900, 1:950 or 1:1000, etc.

[0069] In the embodiments of the present application, the ratio of iridium atoms to hydrogen peroxide is reasonably set to ensure that the hydrolysis reaction product is fully oxidized and to improve the product conversion rate.

[0070] In the embodiment of the present application, the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is set to 1:1 to 1:10. In a specific example, the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc.

[0071] In the implementation of the present application, the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is reasonably set to ensure that the titanium dioxide is fully coated to form a core-shell structure.

[0072] In some embodiments, the hydrolysis reaction and the oxidation reaction comprise the steps of:

[0073] preparing an iridium precursor in aqueous solution;

[0074] adding titanium dioxide into the aqueous solution to prepare a dispersion;

[0075] adding an alkaline substance to the dispersion to carry out a hydrolysis reaction;

[0076] Hydrogen peroxide is added to the hydrolysis reaction system to carry out an oxidation reaction.

[0077] In some embodiments, the hydrolysis reaction time is within 1 hour. Further, the hydrolysis reaction time is 0.5 hours to 1 hour.

[0078] In some embodiments, the oxidation reaction time is 1 h to 6 h. Further, the oxidation reaction time is 2.5 h to 3.5 h.

[0079] In some embodiments, after the oxidation reaction is completed, the method further comprises the following steps:

[0080] The oxidation reaction system is filtered, washed and dehydrated to obtain a precursor of an iridium-based supported catalyst, and then the precursor of the iridium-based supported catalyst is calcined.

[0081] Dehydration treatment includes hot air drying, vacuum drying or heating drying.

[0082] Furthermore, after the oxidation reaction is completed, the method further comprises the following steps:

[0083] The oxidation reaction system is filtered, washed and dried to obtain a precursor of an iridium-based supported catalyst, and then the precursor of the iridium-based supported catalyst is calcined.

[0084] Furthermore, the drying temperature is 60°C to 100°C; and the drying time is 8h to 16h.

[0085] The second aspect of the present application provides an iridium-based supported catalyst, comprising a core body and a shell layer coated outside the core body; the core body comprises TiO2, and the shell layer comprises IrOx , where x=1~2.

[0086] The iridium-based supported catalyst IrO provided in the examples of the present application x @TiO2 is a core-shell structure in which iridium oxide is uniformly coated on the surface of titanium dioxide, and the value of x is 1 to 2, that is, the iridium oxide can be a multivalent iridium oxide. This catalyst can effectively reduce the iridium loading and has a higher catalytic performance.

[0087] In some embodiments, the shell layer has a thickness of 1 nm to 10 nm.

[0088] In the embodiment of the present application, a nanometer-thick iridium oxide shell is formed on the surface of titanium dioxide, which is conducive to forming a uniform conductive network and reducing the load of iridium. In a specific example, the thickness of the shell is 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm and 10nm.

[0089] In some embodiments, based on the total mass of the catalyst, IrO x The mass percentage is 20% to 75%.

[0090] Furthermore, based on the total mass of the catalyst, IrO x The mass percentage is 20% to 40%.

[0091] In some embodiments, the iridium-based supported catalyst is prepared using the above-mentioned preparation method.

[0092] The third aspect of the present application provides a proton exchange membrane water electrolysis membrane electrode, comprising the iridium-based supported catalyst obtained by the above-mentioned preparation method, or comprising the above-mentioned iridium-based supported catalyst.

[0093] The iridium-based catalyst IrO provided in the examples of the present application x @TiO2, the iridium oxide shell fully covers the surface of titanium dioxide, with a thickness of only a few nanometers, which effectively reduces the iridium loading and increases its conductivity. The core-shell catalyst has excellent oxygen evolution performance and excellent electrolysis performance in PEM water electrolysis.

[0094] In a fourth aspect, the present application provides an application of an iridium-based supported catalyst in a water electrolysis reaction, wherein the iridium-based supported catalyst is the iridium-based supported catalyst obtained by the above-mentioned preparation method, or is the above-mentioned iridium-based supported catalyst.

[0095] The iridium-based catalyst IrO provided in the examples of the present application x @TiO2 has excellent electrolytic performance in PEM electrolysis of water.

[0096] Example 1

[0097] This embodiment provides an iridium-based supported catalyst, which is 40% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0098] Step 1: Dissolve 1.39 g of IrCl3 in 150 mL of ultrapure water, then add 1.12 g of TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 5.3 g of hydrogen peroxide and continue the reaction for 3 hours.

[0099] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0100] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 40% IrO x @TiO2-NP.

[0101] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 40% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 40% IrO x @TiO2-NR.

[0102] Example 2

[0103] This embodiment provides an iridium-based supported catalyst, which is 20% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0104] Step 1: Dissolve 1.5 g H2IrCl6 in 150 mL ultrapure water, then add 1.83 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 3.8 g hydrogen peroxide and continue the reaction for 3 hours.

[0105] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0106] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 20% IrO x @TiO2-NP.

[0107] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 20% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 20% IrO x @TiO2-NR.

[0108] Example 3

[0109] This embodiment provides an iridium-based supported catalyst, which is 30% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0110] Step 1: Dissolve 2.5 g H2IrCl6 in 150 mL ultrapure water, then add 4.5 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 5.5 g hydrogen peroxide and continue the reaction for 3 hours.

[0111] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0112] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 30% IrO x @TiO2-NP.

[0113] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 30% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 30% IrO x @TiO2-NR.

[0114] Example 4

[0115] This embodiment provides an iridium-based supported catalyst, which is 60% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0116] Step 1: Dissolve 2.8 g Na2IrCl6 in 150 mL ultrapure water, then add 0.72 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 17.35 g hydrogen peroxide and continue the reaction for 3 hours.

[0117] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0118] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 60% IrO x @TiO2-NP.

[0119] According to the method shown in steps 1 to 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 60% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 60% IrO x @TiO2-NR.

[0120] Example 5

[0121] This embodiment provides an iridium-based supported catalyst, which is 75% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0122] Step 1: Dissolve 4.2 g Na3IrCl6 in 150 mL ultrapure water, then add 0.5 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 8.35 g hydrogen peroxide and continue the reaction for 3 hours.

[0123] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0124] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 30% IrO x @TiO2-NP.

[0125] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 75% IrO x@TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 75% IrO x @TiO2-NR.

[0126] Example 6

[0127] This embodiment provides an iridium-based supported catalyst, which is 50% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0128] Step 1: Dissolve 1.39 g of IrCl3 in 150 mL of ultrapure water, then add 0.75 g of TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 13, and finally add 10.6 g of hydrogen peroxide and continue the reaction for 3 hours.

[0129] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0130] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 50% IrO x @TiO2-NP.

[0131] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst, named 50% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 50% IrO x @TiO2-NR.

[0132] Example 7

[0133] This embodiment provides an iridium-based supported catalyst, which is 20% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0134] Step 1: Dissolve 1.5 g H2IrCl6 in 150 mL ultrapure water, then add 1.83 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 11, and finally add 10.6 g hydrogen peroxide and continue the reaction for 3 hours.

[0135] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0136] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 20% IrO x @TiO2-NP.

[0137] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 20% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 20% IrO x @TiO2-NR.

[0138] Example 8

[0139] This embodiment provides an iridium-based supported catalyst, which is 50% IrO x @TiO2-550 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0140] Step 1: Dissolve 1.39 g of IrCl3 in 150 mL of ultrapure water, then add 0.75 g of TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 10.6 g of hydrogen peroxide and continue the reaction for 3 hours.

[0141] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0142] Step 3: The product obtained in step 2 was calcined at 550°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 50% IrO x @TiO2-NP-550.

[0143] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst, named 50% IrO x @TiO2-NW-550; the iridium-based supported catalyst prepared by replacing TiO2 nanoparticles with TiO2 nanorods is named 50% IrO x @TiO2-NR-550.

[0144] Example 9

[0145] This embodiment provides an iridium-based supported catalyst, which is 50% IrO x@TiO2-450 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0146] Step 1: Dissolve 1.39 g of IrCl3 in 150 mL of ultrapure water, then add 0.75 g of TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 9, and finally add 10.6 g of hydrogen peroxide and continue the reaction for 3 hours.

[0147] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0148] Step 3: The product obtained in step 2 was calcined at 450°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 50% IrO x @TiO2-NP-550.

[0149] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst, named 50% IrO x @TiO2-NW-450; the iridium-based supported catalyst prepared by replacing TiO2 nanoparticles with TiO2 nanorods is named 50% IrO x @TiO2-NR-450.

[0150] Example 10

[0151] This embodiment provides an iridium-based supported catalyst, which is 20% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0152] Step 1: Dissolve 1.5 g H2IrCl6 in 150 mL ultrapure water, then add 1.83 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 11, and finally add 94.8 g (1:1000) hydrogen peroxide and continue the reaction for 3 hours.

[0153] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0154] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 20% IrO x @TiO2-NP.

[0155] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 20% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 20% IrO x @TiO2-NR.

[0156] Embodiment 11

[0157] This embodiment provides an iridium-based supported catalyst, which is 20% IrO x @TiO2 nanoparticles, the value of x is 1 to 2, and the specific preparation method is as follows:

[0158] Step 1: Dissolve 1.5 g H2IrCl6 in 150 mL ultrapure water, then add 1.83 g TiO2 nanoparticles and disperse them evenly under ultrasound. Then use KOH to adjust the pH of the solution to 11, and finally add 47.4 g (1:500) hydrogen peroxide and continue the reaction for 3 hours.

[0159] Step 2: Filter, wash and dry the solution obtained in step 1 to obtain IrO x @TiO2 material precursor;

[0160] Step 3: The product obtained in step 2 was calcined at 350°C for 1 h under air atmosphere to obtain an iridium-based supported catalyst named 20% IrO x @TiO2-NP.

[0161] According to the method shown in step 1 to step 3 above, TiO2 nanowires are used to replace TiO2 nanoparticles to prepare an iridium-based supported catalyst named 20% IrO x @TiO2-NW; TiO2 nanorods were used to replace TiO2 nanoparticles to prepare the iridium-based supported catalyst, named 20% IrO x @TiO2-NR.

[0162] 1. Characterization and Analysis

[0163] 1. Morphology characterization: 40% IrO obtained in Example 1 x @TiO2-NP and 40% IrO obtained in Example 1 x @TiO2-NR, 20% IrO obtained in Example 2 x TEM-mapping of @TiO2-NW Figure 1-Figure 3 As shown, it clearly demonstrates the core-shell structure with the elements evenly distributed on the surface.

[0164] 2. Iridium content detection: The iridium content is mainly determined by TEM-mapping, and the results are as follows Figure 4-Figure 6 As shown, the 40% IrO obtained in Example 1 x @TiO2-NP, 40% IrO obtained in Example 1 x @TiO2-NR and 20% IrO obtained in Example 2 x The iridium contents of @TiO2-NW are 42.48%, 45.51% and 17.8%, respectively.

[0165] 2. Performance Test

[0166] (I) OER catalytic performance test:

[0167] 1.ink configuration:

[0168] Weigh 4 mg of the above samples (40% IrO x @TiO2-NP, 40% IrO obtained in Example 1 x @TiO2-NR and 20% IrO obtained in Example 2 x @TiO2-NW) was placed in a glass container, 500 μl of water and isopropanol were measured respectively, and 15 μl of nafion was added. After ultrasonication for half an hour, 6 μl was measured and dropped on the rotating disk electrode and dried naturally.

[0169] 2. Electrochemical performance test:

[0170] The prepared rotating disk electrode was used as the working electrode, the silver / silver chloride electrode as the reference electrode, and the platinum sheet as the counter electrode. They were activated at 0-1.5 V for 50 cycles and finally tested at 1.1-1.7 V.RHE at a scan rate of 5 mV / s.

[0171] Test results such as Figure 7 Shown: 40% IrO x @TiO2-NP at a current density of 10mA / cm 2 When the overpotential is 315mV; 40% IrO x @TiO2-NR at a current density of 10mA / cm 2 When the overpotential is 325mV; 20% IrO x @TiO2-NW at a current density of 10mA / cm 2 When , its overpotential is 328mV.

[0172] (II) Electrolyzed water performance test:

[0173] 1. Membrane electrode preparation:

[0174] Cathode ink configuration: 0.5 g 50% Pt / C, 4 g water and 36 g isopropanol were weighed in a beaker, stirred at 17000 rpm for 1 h under an emulsifying shearing machine, and then ultrasonically sprayed on a Dongyue 125 μm membrane with a loading of 0.1 mg / cm 2 .

[0175] Anode ink configuration: weigh 0.5 g of the above catalyst (40% IrO x @TiO2-NP, 40% IrO obtained in Example 1 x @TiO2-NR and 20% IrO obtained in Example 2 x @TiO2-NW), 3.2g water and 36.8g isopropanol were placed in a beaker and stirred at 14000rpm for 30min under an emulsifying shearing machine. Then, the anode catalyst was ultrasonically sprayed on the reverse side of the cathode side with a loading of 0.1mg / cm 2 .

[0176] 2 Assembly of electrolytic cell:

[0177] Titanium felt was used as the anode diffusion layer, carbon paper was used as the cathode diffusion layer, PTFE was used as the seal, and the self-made electrode plates and end plates were used to assemble the water-electric device.

[0178] 3. Electrolyzed water performance test:

[0179] PEM electrolytic cell test, such as Figure 8 Specifically, ultrapure water was used, the test temperature was 60-80°C, the proton exchange membrane thickness was 125 μm, the water flow rate was 600 ml / min, and the test process was: when the current density was less than 0.05 A / cm 2 When 0.01A / cm 2 Start with an increment of 0.01; when the current density is less than 0.1A / cm 2 , greater than 0.05A / cm 2 When the current density is less than 0.4A / cm 2 , greater than 0.1A / cm 2 When the current density is less than 1A / cm 2 , greater than 0.4A / cm 2 When the current density is less than 3A / cm 2 , greater than 1A / cm 2 The current density was increased by 0.2 and maintained at each current density for 50 seconds.

[0180] Test results: Fig. 9 As shown, with 40% IrO x@The electrolytic cell with TiO2-NP as catalyst, at a current density of 1A / cm 2 , 2A / cm 2 When the electrolysis voltage is 1.66V, 1.79V; with 40% IrO x @TiO2-NR is used as the catalyst in the electrolytic cell, at a current density of 1A / cm 2 , 2A / cm 2 When the electrolysis voltage is 1.67V, 1.8V; with 20% IrO x @TiO2-NW is used as the catalyst in the electrolytic cell. At a current density of 1A / cm 2 , 2A / cm 2 When , the electrolysis voltage is 1.64V and 1.77V.

[0181] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing an iridium-based supported catalyst, characterized in that: include: Using titanium dioxide as a carrier, hydrolyzing an iridium precursor with an alkaline substance, and then oxidizing the hydrolysis product with hydrogen peroxide to obtain a precursor of an iridium-based supported catalyst; The precursor of the iridium-based supported catalyst is calcined in an atmosphere of oxygen to prepare an iridium-based supported catalyst IrO x @TiO2, where x = 1 to 2, IrO x As a shell layer coated on the surface of TiO2 core.

2. The method for preparing an iridium-based supported catalyst according to claim 1, wherein The raw materials meet at least one of the following (1) to (3): (1) The iridium precursor includes at least one of IrCl3, Na3IrCl6, Na2IrCl6 and H2IrCl6; (2) the alkaline substance comprises at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate and lithium carbonate; (3) The morphology of the titanium dioxide includes at least one of titanium dioxide nanoparticles, titanium dioxide nanowires and titanium dioxide nanorods.

3. The method for preparing an iridium-based supported catalyst according to claim 1 or 2, wherein: In the step of the hydrolysis reaction: the parameter pH value is controlled to be 9-13.

4. The method for preparing an iridium-based supported catalyst according to claim 1 or 2, wherein: In the calcination step, the control parameters meet the following requirements: The calcination temperature is 250° C. to 450° C.; and / or the calcination time is 0.5 h to 2 h.

5. The method for preparing an iridium-based supported catalyst according to claim 1 or 2, characterized in that: The molar mass ratio of iridium atoms to hydrogen peroxide in the iridium precursor is 1:20 to 1:1000; and / or the molar mass ratio of iridium atoms to titanium dioxide in the iridium precursor is 1:1 to 1:

10.

6. The method for preparing an iridium-based supported catalyst according to claim 1 or 2, characterized in that: The hydrolysis reaction and the oxidation reaction comprise the steps of: preparing an aqueous solution of the iridium precursor; adding the titanium dioxide into the aqueous solution to prepare a dispersion; adding an alkaline substance to the dispersion to perform a hydrolysis reaction; Hydrogen peroxide is added to the hydrolysis reaction system to carry out an oxidation reaction.

7. An iridium-based supported catalyst, characterized in that It comprises a core body and a shell layer coated outside the core body; the core body comprises TiO2, and the shell layer comprises IrO x , where x=1~2.

8. An iridium-based supported catalyst according to claim 7, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6, IrO x The mass percentage is 20% to 75%.

9. A proton exchange membrane water electrolysis membrane electrode, characterized in that: The invention comprises an iridium-based supported catalyst obtained by the preparation method according to any one of claims 1 to 6, or comprises an iridium-based supported catalyst according to claim 7 or 8.

10. Use of an iridium-based supported catalyst in a water electrolysis reaction, wherein the iridium-based supported catalyst is an iridium-based supported catalyst obtained by the preparation method according to any one of claims 1 to 6, or is an iridium-based supported catalyst according to claim 7 or 8.

Citation Information

Patent Citations

  • Iridium-based anti-antipolar catalyst and preparation method and application thereof

    CN116682981A

Cited By

  • Preparation method and application of supported iridium-based OER catalyst

    CN119615269A

  • Preparation method and application of supported iridium-based OER catalyst

    CN119615269B