Janus cotton fabric with directional perspiration and photo-thermal evaporation functions and preparation method of Janus cotton fabric
By combining photothermal and hydrophobic layers in Janus cotton fabrics, the directional transportation and rapid evaporation of sweat is achieved using photothermal effects and Janus characteristics, the problem of insufficient sweat management in traditional fabrics during outdoor exercises is solved, ensuring the comfort of the body and Moisture and heat management effect.
Patent Information
- Application Number
- CN202411197536.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Traditional fabrics are difficult to effectively manage sweat during strenuous exercise outdoors, resulting in dampness, increased discomfort and reduced cooling effect. Janus fabrics may reach saturation when sweating a lot, affecting comfort.
Using Janus cotton fabric with photothermal and hydrophobic layers, sweat is transported in a directional direction on the hydrophobic side to the superhydrophilic side by photothermal effect, and evaporation is accelerated through the photothermal layer, combining photothermal conversion and Janus characteristics to achieve rapid evaporation.
Ensure effective sweating and moisture-heat management during high-intensity physical activities, maintain body comfort, prevent hypothermia, and remove excessive sweating through solar-powered evaporation.
Smart Images

Figure CN118957990A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functionalized Janus fabric and comfort of personal moisture and heat management, and in particular to a Janus cotton fabric with directional perspiration and photothermal evaporation functions and a preparation method thereof. Background Art
[0002] The comfort of personal heat and moisture management is mainly related to perspiration and temperature regulation. However, traditional fabrics have significant limitations in perspiration and moisture management. Especially during strenuous outdoor exercise, people tend to sweat a lot, causing clothes to quickly become wet. This not only increases the discomfort of the human body, but also significantly reduces the cooling effect of the clothing. At the same time, due to the limited moisture transfer performance of traditional fabrics, it is difficult to effectively discharge sweat from the skin surface, further affecting the comfort of wearing.
[0003] To solve this problem, fabrics need to meet two major requirements to achieve effective moisture and heat management when sweating a lot: one is to be able to transport sweat from the skin to the environment in a directional manner, and the other is to be able to quickly evaporate the excess sweat accumulated in the clothing. Therefore, smart textiles with adjustable transmission properties have gradually attracted attention and have shown great potential in regulating the humidity and temperature of the microenvironment around human skin. Among them, Janus fabric, as an innovative material with asymmetric wettability, provides an effective solution for directional sweat transport. This fabric is cleverly composed of thin hydrophobic and hydrophilic layers, allowing water to be efficiently transferred from the hydrophobic side to the hydrophilic side while effectively preventing reverse transmission. However, it is worth noting that in the case of heavy sweating, Janus fabric may reach saturation, resulting in its liquid transmission capacity being blocked, and it may not be able to continuously and effectively discharge sweat from the skin surface, thus affecting the body's comfort. Summary of the invention
[0004] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a Janus cotton fabric with directional perspiration and photothermal evaporation functions. The Janus cotton fabric provided by the present invention combines the conversion of light and heat with the Janus characteristics. The photothermal effect generated by the photothermal coating quickly evaporates the sweat that is directional transported from the internal hydrophobic surface to the external super-hydrophilic surface, thereby ensuring comfort during physical activities and promoting personal moisture and heat management, making it an ideal choice for moisture and heat management in high-intensity sports activities.
[0005] The second object of the present invention is to provide a method for preparing Janus cotton fabric with directional perspiration and photothermal evaporation functions.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention discloses a Janus cotton fabric with directional perspiration and photothermal evaporation functions. The Janus cotton fabric comprises a cotton fabric base, photothermal layers arranged on both sides of the cotton fabric base, and a hydrophobic layer arranged on the raised part inside the cotton fabric base, wherein the hydrophobic layer is located on the surface of the photothermal layer; and the inner side of the Janus cotton fabric is a concave-convex structure.
[0008] The Janus cotton fabric provided by the present invention combines the conversion of light and heat with the Janus property. Under the action of the Janus property, the directional transport of sweat from the hydrophobic side to the hydrophilic side can be achieved. The photothermal effect generated by the photothermal layer can generate a local high temperature of up to 39.8°C under light, and can accelerate the rate of unidirectional drainage by promoting the evaporation rate, thereby ensuring comfort during physical activities. In the present invention, the inner side of the Janus cotton fabric refers to the contact surface with the skin during actual application.
[0009] In a preferred embodiment, the photothermal layer is a polyacrylic acid (PAA) / polypyrrole (PPy) nanoparticle composite coating.
[0010] In a preferred embodiment, the hydrophobic layer is a PDMS membrane.
[0011] In a preferred embodiment, the convex part of the inner side of the Janus cotton fabric is hydrophobic, the concave part is hydrophilic, and the outer side of the Janus cotton fabric is super-hydrophilic. The inner side of the Janus cotton fabric of the present invention has a concave-convex structure at a microscopic level, wherein the convex part is hydrophobic due to the provision of a hydrophobic layer, and the concave part is hydrophilic. This hydrophobic-hydrophilic structure has a wettability gradient, generates a Laplace pressure difference, drives the directional transport of liquid, and further accelerates the discharge of sweat.
[0012] The invention discloses a preparation method of a Janus cotton fabric with directional perspiration and photothermal evaporation functions. The method comprises the following steps: pretreating a cotton fabric to obtain a pretreated cotton fabric, then soaking the pretreated cotton fabric in a silane solution to obtain a silane-treated cotton fabric, then soaking the silane-treated cotton fabric in a polyacrylic acid (PAA) solution and a polypyrrole (PPy) nanoparticle solution in sequence to obtain a cotton fabric with a photothermal layer, then wetting the cotton fabric with the photothermal layer with a sodium chloride aqueous solution, finally dropping a mixed solution containing PDMS on the inner surface of the cotton fabric with the photothermal layer, and drying the cotton fabric to obtain the Janus cotton fabric with directional perspiration and photothermal evaporation functions.
[0013] The preparation method of the present invention uses cotton fabric as a substrate, which has excellent hydrophilicity. The present invention first further improves the hydrophilicity of the cotton fabric through pretreatment, and then uses a silane solution to treat the cotton fabric so that the cotton fabric is modified with a positive charge. Then, positively charged polypyrrole (PPy) nanoparticles and negatively charged polyacrylic acid (PAA) are used as materials for assembly through electrostatic attraction. Finally, negatively charged PAA and positively charged PPy nanoparticle coatings are prepared as photothermal surfaces through LBL assembly. Subsequently, a mixed solution of polydimethylsiloxane (PDMS) and a curing agent in n-hexane was dropped on the inner surface of the cotton fabric with a photothermal layer moistened with an aqueous sodium chloride solution. By utilizing the immiscible characteristics of the aqueous solution and n-hexane, the volatility of n-hexane, and the fact that the density of the aqueous sodium chloride solution is greater than that of polydimethylsiloxane (PDMS), the PDMS was successfully aggregated and deposited on the raised part on one side of the cotton fabric, forming a hydrophobic-hydrophilic structure with the recessed part, thereby flexibly realizing the one-sided hydrophobic modification of the cotton fabric. The outer surface was not hydrophobically modified and still maintained super hydrophilicity, thereby obtaining a hydrophobic-hydrophilic alternating structure on the inside and a super hydrophilic structure on the outside.
[0014] In a preferred embodiment, the process of pretreating the cotton fabric is to soak the cotton fabric in a NaOH aqueous solution with a pH of 8-10, control the soaking temperature to be 60-90° C., and soak for 1-2 hours.
[0015] In the actual operation process, after the cotton fabric is soaked, it is taken out with tweezers and cleaned with anhydrous ethanol and ultrapure water under ultrasonic conditions to clean off the excess NaOH on the surface of the initial cotton fabric. Then, it is blown dry with a hair dryer to obtain the pretreated cotton fabric for standby use. In the present invention, the initial cotton fabric is soaked with a strong alkali to activate the hydroxyl groups on the surface of the initial cotton fabric so that the initial cotton fabric exhibits better hydrophilicity; at the same time, the roughness of the surface of the initial cotton fabric can be increased to facilitate better adhesion of PDMS to the surface of the initial cotton fabric.
[0016] In a preferred embodiment, the silane solution is a mixture of water, acetic acid solution and 3-aminopropyltriethoxysilane, wherein the mass fraction of 3-aminopropyltriethoxysilane in the silane solution is 1-5wt%, and the volume ratio of water to acetic acid solution is 500ml:100-500μl.
[0017] Further preferably, the pH of the acetic acid solution is 2-4.
[0018] In a preferred embodiment, the pretreated cotton fabric is immersed in the silane solution for 1-2 hours and then dried to obtain the silane-treated cotton fabric.
[0019] In the actual operation process, after the pre-treated cotton fabric is immersed in the silane solution, it is taken out with tweezers and rinsed in ethanol, and then heated and dried with a hair dryer to make the cotton fabric completely dry and set aside. The purpose is to make the surface of the cotton fabric have a positive charge.
[0020] In a preferred embodiment, the mass fraction of polyacrylic acid (PAA) in the PAA solution is 1-5 wt %. In actual operation, taking the preparation of 1% polyacrylic acid (PAA) solution as an example, 1 g of polyacrylic acid is weighed and added into a beaker of 100 ml ultrapure water.
[0021] In a preferred embodiment, the polypyrrole (PPy) nanoparticle solution is obtained by dissolving PVA in water to obtain a PVA solution, then adding ferric chloride hexahydrate to the PVA solution to obtain a mixed solution, and then adding pyrrole to the mixed solution to undergo a polymerization reaction to obtain the PPy nanoparticle solution.
[0022] In the PVA solution, the mass fraction of PVA is 1-3.5wt%;
[0023] The solid-liquid mass volume ratio of the ferric chloride hexahydrate to water is 0.5-2g:100ml;
[0024] The volume ratio of pyrrole to water is 0.5-2:100ml.
[0025] In a preferred embodiment, the silane-treated cotton fabric is immersed in a polyacrylic acid (PAA) solution, taken out after 5-30 minutes, and then immersed in a polypyrrole (PPy) nanoparticle solution for 5-30 minutes and dried to obtain a cotton fabric with a photothermal layer.
[0026] In the actual operation process, the prepared pretreated cotton fabric is immersed in the PAA solution, taken out after soaking, and the wetted cotton fabric is suspended in the air to form a thin water film on its surface. Then it is immersed in the PPy solution and kept evenly immersed. It is taken out and placed in an electric heated blast drying oven for drying for 0.5 hours at a temperature of 70°C. After complete drying, a cotton fabric with a photothermal layer is obtained.
[0027] In a preferred embodiment, the mass fraction of sodium chloride in the sodium chloride aqueous solution is ≤26.4%, preferably 9-26.4%, and more preferably 18-26.4%. The inventors found that within the above range, as the content of sodium chloride increases, the density difference between PDMS and the sodium chloride aqueous solution increases, and PDMS is more concentrated on the raised part of one side of the cotton fabric, and the penetration time of water droplets from the hydrophobic side to the hydrophilic side is accelerated, thereby enhancing the Janus effect of the cotton fabric.
[0028] In a preferred embodiment, the amount of sodium chloride aqueous solution added to each 4cmX4cm cotton fabric is 100-400μl, preferably 250-400μl. The amount of sodium chloride aqueous solution added is controlled within the above range, and the performance of the cotton fabric finally obtained is optimal.
[0029] In a preferred embodiment, the PDMS-containing mixed solution is obtained by mixing polydimethylsiloxane (PDMS), a curing agent, and n-hexane, wherein the mass ratio of PDMS to the curing agent is 0.8-1:0.1, and the solid-liquid mass volume ratio of PDMS to n-hexane is 0.06-1g:10ml;
[0030] In actual operation, the mixed solution containing PDMS can be obtained by adding 0.7 g PDMS and 0.07 g curing agent into 10 mL n-hexane and stirring for 10 min to obtain the PDMS solution.
[0031] In the present invention, the type of curing agent is not limited, and any curing agent for PDMS described in the prior art can be used.
[0032] Further preferably, the curing agent is commercially available Dow Corning 184. The Dow Corning 184 curing agent can be used together with the PDMS to form a network structure, so that the PDMS and the curing agent harden when mixed.
[0033] In the actual operation process, the cotton fabric with the photothermal layer is clamped and fixed on the manual translation stage. The NaCl aqueous solution is first evenly dropped on the surface of the cotton fabric with the photothermal layer obtained above with a pipette to form a layer of water film. Then the PDMS mixed solution is evenly dropped on the water film with a pipette. When dropping the sodium chloride aqueous solution to form the water film and dropping the PDMS mixed solution on it, pay attention to the experimental operation and do not puncture the water film formed by the sodium chloride aqueous solution to prevent PDMS from penetrating into the other side of the cotton fabric. After the n-hexane is completely evaporated, it is placed under a hair dryer for heating treatment. After the cotton fabric is completely dried, the coated cotton fabric is obtained.
[0034] Finally, the coated cotton fabric is placed in an electric hot air drying oven for drying, and after drying, is placed in ultrapure water for ultrasonic cleaning to obtain the Janus cotton fabric with directional perspiration and photothermal evaporation functions;
[0035] The purpose of the drying treatment is to make the PDMS better solidify and adhere to the surface of the coated cotton fabric, and the purpose of the ultrasonic cleaning is to clean the sodium chloride particles on the surface of the coated cotton fabric. The drying treatment temperature is 90°C, the time is 0.5h, and the ultrasonic cleaning time is 1min.
[0036] In a preferred embodiment, the cotton fabric is kept horizontal during the drying process. After the n-hexane is completely volatilized, the cotton fabric is placed under a hair dryer for heating. During this process, the cotton fabric is kept horizontal, otherwise the aggregation effect of PDMS will be affected.
[0037] Principles and advantages
[0038] The present invention provides a Janus cotton fabric with directional perspiration and photothermal evaporation functions. The Janus cotton fabric comprises a cotton fabric base, a photothermal layer arranged on both sides of the cotton fabric base, and a hydrophilic layer arranged on the outer side of the cotton fabric base, wherein the hydrophilic layer is located on the surface of the photothermal layer; the inner side of the Janus cotton fabric is a concave-convex structure, wherein the convex part of the inner side of the Janus cotton fabric is hydrophobic, the concave part is hydrophilic, and the outer side of the Janus cotton fabric is super hydrophilic.
[0039] The Janus cotton fabric provided by the present invention combines the conversion of light and heat with the Janus property. The photothermal effect generated by the photothermal layer quickly evaporates the sweat that is directionally transported from the internal hydrophobic surface to the external super-hydrophilic surface, thereby ensuring comfort during physical activities.
[0040] The preparation method of the present invention first constructs a photothermal surface composed of photothermal nanomaterials (polypyrrole (PPy) nanoparticles) and polyelectrolyte (polyacrylic acid) on the surface of a cotton fabric substrate. In the present invention, the pretreated cotton fabric is first treated with a silane solution so that the cotton fabric is modified with a positive charge. Then, the positively charged polypyrrole (PPy) nanoparticles and the negatively charged polyacrylic acid (PAA) are assembled as materials through electrostatic attraction. Finally, the negatively charged PAA and the positively charged PPy nanoparticle coating are prepared as the photothermal surface through LBL assembly.
[0041] However, the hydrophobic-hydrophilic structure is reconstructed. In the present invention, a mixed solution of polydimethylsiloxane (PDMS) and a curing agent in n-hexane is dropped on the surface of a cotton fabric having a photothermal layer moistened by a sodium chloride aqueous solution. By utilizing the immiscible characteristics of the aqueous solution and n-hexane, the volatility of n-hexane, and the density of the sodium chloride aqueous solution being greater than that of polydimethylsiloxane (PDMS), the PDMS is successfully aggregated and deposited on the raised portion on one side of the cotton fabric to form a hydrophobic-hydrophilic structure with the recessed portion, thereby flexibly realizing the one-sided hydrophobic modification of the cotton fabric.
[0042] In the process of preparing the hydrophobic-hydrophilic structure, the present invention, on the one hand, uses sodium chloride particles to increase the density of the aqueous solution, because the density of polydimethylsiloxane (PDMS) is slightly smaller than the density of water, and due to the action of capillary force, on the water film on the surface of the cotton fabric, PDMS will climb from the concave part in the center of the water film to the surrounding convex part. On the other hand, by heating and drying, a temperature gradient is formed on the surface of the water film. In addition, because the aqueous solution of the convex part on one side of the cotton fabric is closer to the cotton fiber, the evaporation rate of the part close to the fiber is fast, and as the n-hexane evaporates, the evaporation absorbs heat, so the convex part has a lower temperature and a higher surface tension than the concave part. After the aqueous solution is completely heated and evaporated, finally, PDMS will gather on the convex part of the cotton fabric, so that the convex part has hydrophobicity, while the concave part has a hydrophilic structure, thereby forming a hydrophobic-hydrophilic structure with the concave part.
[0043] The method provided by the present invention is simple to operate, easy to implement, and will not cause secondary pollution to the environment. The prepared photothermal coating of the Janus cotton fabric with directional perspiration and photothermal evaporation functions shows good photothermal performance, and the coating can convert solar energy into thermal energy. The coating manufactured by LBL assembly has the advantages of simplicity and low cost; the hydrophobic gradient of the prepared Janus cotton fabric with directional perspiration and photothermal evaporation functions decreases from the hydrophobicity of the dripped liquid side to the superhydrophilicity of the non-dripped liquid side, and the modified Janus cotton fabric with directional perspiration and photothermal evaporation functions has a hydrophobic-hydrophilic structure on one side and a superhydrophilic structure on the other side; the Janus cotton fabric with directional perspiration and photothermal evaporation functions can perspire in a directional manner through the Janus structure, and remove excess sweat and keep the skin dry through solar evaporation. In addition, it also helps to keep the skin temperature within a normal range and prevent hypothermia caused by excessive sweating; the solar-driven evaporation achieved by the photothermal coating provides a driving force for the directional transport of sweat from the internal hydrophobic surface to the external superhydrophilic surface, and these characteristics can ensure comfort during physical activities. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention is a process flow chart of a method for preparing Janus cotton fabric with directional perspiration and photothermal evaporation functions.
[0045] Figure 2 This is a schematic diagram of the structure of the cotton fabric prepared in Example 1.
[0046] Figure 3 Schematic diagram of the preparation process of the polypyrrole nanoparticle solution in Example 1.
[0047] Figure 4Schematic diagram of the preparation process of the photothermal layer composed of photothermal nanomaterials and polyelectrolytes on cotton fabric in Example 1; positively charged polypyrrole (PPy) nanoparticles and negatively charged polyacrylic acid (PAA) were assembled by electrostatic attraction, and the substrate was initially modified with positively charged chemicals. Subsequently, negatively charged PAA and positively charged PPy nanoparticle coatings were prepared by LBL assembly.
[0048] Figure 5 This is a schematic diagram of the preparation principle of the hydrophobic-hydrophilic phase structure of the Janus cotton fabric in Example 1; the principle is capillary-driven: the added sodium chloride particles are to increase the density of the aqueous solution, and because the density of polydimethylsiloxane (PDMS) is slightly smaller than the density of water, due to the action of capillary force, on the water film on the surface of the cotton fabric, the PDMS will climb from the concave part in the center of the water film to the surrounding convex part.
[0049] Figure 6 The figure is a flow chart of the preparation of hydrophobic / hydrophilic interphase-super hydrophilic structure of Janus cotton fabric in Example 1; hot air heating and drying are used to form a temperature gradient on the surface of the water film. In addition, because the aqueous solution of the raised part on one side of the cotton fabric is closer to the cotton fiber, the evaporation rate of the part close to the fiber is fast, and as the n-hexane evaporates, the evaporation absorbs heat, so the raised part has a lower temperature and higher surface tension than the recessed part. After the aqueous solution is completely heated and evaporated, PDMS will eventually gather on the raised part of the cotton fabric to form a hydrophobic-hydrophilic structure with the recessed part, and the other side of the cotton fabric is a super hydrophilic structure.
[0050] Figure 7 Schematic diagram of the directional transport function of Janus cotton fabric in Example 2.
[0051] Figure 8 This is a photothermal heating effect diagram of the Janus cotton fabric in Example 3 under the irradiation of a xenon lamp light source of 350nm-780nm.
[0052] Fig. 9 This is the evaporation rate diagram of Janus cotton fabric in Example 4.
[0053] Fig.10 This is the evaporation mass diagram of Janus cotton fabric in Example 4. DETAILED DESCRIPTION
[0054] Example 1
[0055] A method for preparing Janus cotton fabric with directional perspiration and photothermal evaporation functions, such as Figure 1 As shown, it includes the following steps:
[0056] 1) Cut the initial cotton fabric of 4cmX4cm, such as Figure 2As shown, the initial cotton fabric is completely immersed in NaOH with a pH value of 10 and placed in a water bath for 1 hour at a temperature of 60°C. After 1 hour, the initial cotton fabric is taken out with tweezers and cleaned with anhydrous ethanol and ultrapure water under ultrasonic conditions to clean off the excess NaOH on the surface of the initial cotton fabric, and then dried with a hair dryer to obtain the pretreated cotton fabric for later use;
[0057] 2) First, prepare a polyvinyl alcohol (PVA) precursor solution. Dissolve 1g of PVA in 100ml of water and heat to 90°C with magnetic stirring to form a transparent solution. After the PVA solution is cooled to room temperature, add 1g of ferric chloride hexahydrate. Then, slowly inject 1ml of pyrrole under magnetic stirring. The solution immediately turns black and is stored overnight to obtain a polypyrrole (PPy) nanoparticle solution, such as Figure 3 As shown, spare;
[0058] 3) Weigh 1 g of polyacrylic acid and add it into a beaker containing 100 ml of ultrapure water to obtain a PAA (polyacrylic acid) solution (1 wt%);
[0059] 4) Measure 500 ml of deionized water, 100 ul of acetic acid (pH=3) and 1 wt% of 3-aminopropyltriethoxysilane, and mix the three solutions to obtain a silane solution;
[0060] 5) The pretreated cotton fabric was immersed in the silane solution for 1 hour. After immersion, it was taken out with tweezers and placed in anhydrous ethanol for cleaning, and then heated and dried with a hair dryer to make the cotton fabric completely dry for use; the prepared cotton fabric was immersed in the PAA solution for 5 minutes, and taken out after immersion. The wetted cotton fabric was suspended in the air to form a thin layer of water film on its surface, and then immersed in the PPy solution for 5 minutes, maintaining uniform immersion, and then taken out and placed in an electric heating blast drying oven for drying for 0.5 hours at a temperature of 70°C. After complete drying, a cotton fabric with a photothermal layer was obtained, such as Figure 4 As shown;
[0061] 6) Weigh 0.07 g PDMS and 0.007 g curing agent into a 15 ml test tube, add 10 ml n-hexane, and stir with a magnetic stirrer to obtain a PDMS mixed solution;
[0062] 7) Weigh 2.64 g NaCl into a 50 ml test tube, add 10 ml ultrapure water, and stir with a magnetic stirrer to obtain a NaCl aqueous solution;
[0063] 8) Clamp and fix the cotton fabric with the photothermal layer on the manual displacement stage, first use a pipette to evenly drop 400 μl of NaCl aqueous solution on the surface of the cotton fabric with the photothermal layer obtained above to form a water film, then use a pipette to evenly drop 80 μl of PDMS mixed solution on the water film, after the n-hexane is completely volatilized, place it under a hair dryer for heating for 2 minutes, and after the cotton fabric is completely dried, obtain the coated cotton fabric;
[0064] 9) The coated cotton fabric was placed in an electric blast drying oven at 90° C. for drying for 0.5 h. After drying, the coated cotton fabric was placed in ultrapure water and ultrasonically cleaned in an ultrasonic cleaning machine for 1 min to obtain the Janus cotton fabric with directional perspiration and photothermal evaporation functions.
[0065] Performance Testing
[0066] 1) Hydrophilic and hydrophobic performance testing
[0067] This embodiment provides a unidirectional transport performance test of a Janus cotton fabric prepared by a method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions. By dropping droplets on different sides of the Janus cotton fabric, the water transport behavior on it is studied. The dynamic transport process of droplets on the Janus cotton fabric is monitored by a contact angle tester. Figure 7 As shown in the figure, when the hydrophobic side is placed upward, the droplet is on the hydrophobic side, the droplet quickly passes through the hydrophilic side, and wets the hydrophilic side within 22 seconds, leaving a dry hydrophobic surface. On the contrary, when the hydrophilic side is placed upward, the droplet quickly spreads on the hydrophilic surface while being blocked by the hydrophobic side.
[0068] The initial water contact angle of one side of the Janus cotton fabric prepared in this example was 136°, showing high hydrophobicity, and the water contact angle of the other side was 0°, showing super hydrophilicity. Figure 7 The process of water droplet transport from the hydrophobic side to the superhydrophilic side and vice versa on Janus cotton fabric is shown. Figure 7 It can be seen that Janus cotton fabric has the function of unidirectional transport of water droplets. The water droplets are spontaneously transported from the hydrophobic side to the superhydrophilic side at 22s, but are blocked by the superhydrophilic side in the opposite direction and cannot be transported.
[0069] 2) Photothermal heating performance test
[0070] The photothermal heating of Janus cotton fabric was tested, and the temperature rise change of Janus cotton fabric was measured by a thermal imager. Ordinary cotton fabric and Janus cotton fabric with a photothermal layer were soaked in water for 20 seconds, placed flat on a constant temperature heating table at 37.5℃, irradiated with a 350nm-780nm xenon light source for 1 minute, and the temperature change was recorded by a thermal imager. Ordinary cotton fabric and Janus cotton fabric with a photothermal layer were irradiated with a 350nm-780nm xenon light source for 1 minute, and the temperature change was recorded by a thermal imager, as shown in Figure 2. Figure 8 As shown, ordinary cotton fabrics do not show obvious warming effect, while the temperature of Janus cotton fabrics with a photothermal layer rises rapidly, the temperature can reach 39.8°C, and it also has a photothermal effect after wetting.
[0071] 3) The Janus cotton fabric of Example 1 was tested for the rate of water evaporation from the surface of simulated human skin.
[0072] Use a syringe to draw 400 microliters of water droplets on 4×4 cm 2 The hydrophilic surfaces of ordinary cotton fabric, Janus cotton fabric and photothermal Janus cotton fabric were undisturbed for a certain period of time to allow the various cotton fabrics to absorb water to a balance. Subsequently, the fabrics were placed flat on a 37.5°C constant temperature heating table with the hydrophilic side facing up and the hydrophobic side facing down, and a 350nm-780nm xenon light source was placed above the cotton fabrics. Under the irradiation of the 350nm-780nm xenon light source, the mass of the cotton fabric was recorded on a balance for 4 minutes. After 4 minutes of irradiation with the xenon light source, the mass change of the photothermal Janus cotton fabric group was the largest, with a mass decrease of 0.012g cm -2 The mass of the ordinary cotton fabric group decreased by 0.008 g cm -2 The mass loss of the photothermal Janus cotton fabric group is 1.5 times that of the ordinary cotton fabric group. Fig. 9 In addition, the evaporation rate of the Janus cotton fabric group was 0.181 g cm -2 h -1 , higher than the 0.117 g cm of the ordinary cotton fabric group -2 h -1 ,like Fig.10 As shown, it has the ability of photothermal conversion, which can absorb sunlight and convert it into heat, accelerating the evaporation process of water.
[0073] When other conditions were the same as those in Example 1, only the content of sodium chloride and the amount of sodium chloride aqueous solution were changed. The directional transport effect of the obtained Janus cotton fabric was as shown in Table 1.
[0074] Table 1 Effect of different sodium chloride contents and the amount of sodium chloride aqueous solution dropped on the directional transport effect of Janus cotton fabric.
[0075]
[0076] It can be seen from Table 1 that as the sodium chloride content increases, the water droplet transmission time shortens, indicating that the directional transport effect of the Janus cotton fabric is enhanced; at the same time, as the amount of sodium chloride aqueous solution drops increases, the curvature of the water film on one side of the Janus cotton fabric decreases, and PDMS is more likely to gather on the convex part, so that the stronger the hydrophobicity of this side of the Janus cotton fabric, the greater the difference in wettability on both sides of the Janus cotton fabric, resulting in a stronger directional transport effect of the Janus cotton fabric; the second drop of water has a shorter transmission time than the first drop of water, indicating that the prepared Janus cotton fabric achieves the Janus effect; the less the amount of sodium chloride aqueous solution drops, the greater the curvature of the water film, the more difficult it is for PDMS to gather on the convex part, the worse the directional transport effect of the Janus cotton fabric, resulting in a longer water drop transmission time; the lower the sodium chloride content, the smaller the density difference between the sodium chloride aqueous solution and PDMS, and the more difficult it is for PDMS to climb to the convex part, thereby affecting the hydrophobicity of the Janus cotton fabric, resulting in a worse directional transport effect of the Janus cotton fabric and a longer water drop transmission time.
Claims
1. A Janus cotton fabric with directional perspiration and photothermal evaporation functions, characterized in that: The Janus cotton fabric consists of a cotton fabric base, a photothermal layer arranged on the double-side surfaces of the cotton fabric base, and a hydrophobic layer arranged on the raised part inside the cotton fabric base, wherein the hydrophobic layer is located on the surface of the photothermal layer; the inner side of the Janus cotton fabric is a concave-convex structure.
2. The Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 1, characterized in that: The photothermal layer is a PAA / PPy nanoparticle composite coating; The hydrophobic layer is a PDMS membrane.
3. The Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 1 or 2, characterized in that: The convex part on the inner side of the Janus cotton fabric has hydrophobicity, the concave part has hydrophilicity, and the outer side of the Janus cotton fabric has super hydrophilicity.
4. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to any one of claims 1 to 3, characterized in that: The cotton fabric is pretreated to obtain a pretreated cotton fabric, and then the pretreated cotton fabric is immersed in a silane solution to obtain a silane-treated cotton fabric, and then the silane-treated cotton fabric is immersed in a PAA solution and a PPy nanoparticle solution in sequence to obtain a cotton fabric with a photothermal layer, and then the cotton fabric with the photothermal layer is wetted with a sodium chloride aqueous solution, and finally a mixed solution containing PDMS is dropped on the inner surface of the cotton fabric with the photothermal layer, and dried to obtain a Janus cotton fabric with directional perspiration and photothermal evaporation functions.
5. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: The process of pretreating the cotton fabric is to soak the cotton fabric in a NaOH aqueous solution with a pH value of 8-10, control the soaking temperature to be 60-90° C., and soak for 1-2 hours.
6. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: The silane solution is prepared by mixing water, acetic acid solution and 3-aminopropyltriethoxysilane, wherein the mass fraction of 3-aminopropyltriethoxysilane in the silane solution is 1-5wt%, and the volume ratio of water to acetic acid solution is 500ml:100-500μl; The pH of the acetic acid solution is 2-4. The pretreated cotton fabric was immersed in the silane solution for 1-2 hours and then dried to obtain the silane-treated cotton fabric.
7. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: In the PAA solution, the mass fraction of PAA is 1-5wt%; The process of obtaining the PPy nanoparticle solution is as follows: PVA is dissolved in water to obtain a PVA solution, then ferric chloride hexahydrate is added to the PVA solution to obtain a mixed solution, and pyrrole is added to the mixed solution to undergo a polymerization reaction to obtain the PPy nanoparticle solution. In the PVA solution, the mass fraction of PVA is 1-3.5wt%; The solid-liquid mass volume ratio of the ferric chloride hexahydrate to water is 0.5-2g:100ml; The volume ratio of pyrrole to water is 0.5-2:100ml; The silane-treated cotton fabric is immersed in the PAA solution, taken out after 5-30 minutes, and then immersed in the PPy nanoparticle solution for 5-30 minutes and dried to obtain the cotton fabric with the photothermal layer.
8. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: The mass fraction of sodium chloride in the sodium chloride aqueous solution is ≤26.4%; The amount of sodium chloride aqueous solution added per 4cmX4cm cotton fabric is 100-400μl.
9. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: The method for obtaining the PDMS-containing mixed liquid is as follows: PDMS, a curing agent and n-hexane are mixed, wherein the mass ratio of PDMS to the curing agent is 0.8-1:0.1, and the solid-liquid mass volume ratio of PDMS to n-hexane is 0.06-1g:10ml.
10. The method for preparing a Janus cotton fabric with directional perspiration and photothermal evaporation functions according to claim 4, characterized in that: During the drying process, the cotton fabric is kept horizontal.
Citation Information
Patent Citations
Hydrophobic spherulite, hydrophobic material, hydrophobic composite material, Janus composite material as well as preparation methods and application thereof
CN112900081A
Janus fabric with one-way droplet permeability and preparation method of Janus fabric
CN113564918A
Photo-thermal self-pumping fabric and preparation method thereof
CN115195221A
PH response Janus fabric based on water-based organosilicon polyurethane and preparation method of PH response Janus fabric
CN116988305A
Method and device for detecting in real time a secreted compound and the secretion target, and uses thereof
US20180045711A1
Cited By
Antibacterial functional fabric capable of directionally transporting sweat in response to ultraviolet light as well as preparation method and application of antibacterial functional fabric
CN119777162A
A bacteriostatic functional fabric for ultraviolet-responsive directional sweat transport, and its preparation method and application
CN119777162B