Method for degrading antibiotics in water body by activating hydrogen peroxide with iron-doped ZSM5 type zeolite
Through the preparation and application of iron-doped ZSM5 zeolite catalyst, the problems of low antibiotic degradation efficiency and insufficient catalyst stability in the prior art were solved, and efficient and environmentally friendly antibiotic degradation effect was achieved, and reactive oxygen species were generated through hydrogen peroxide activation. Species overcome the problems of catalyst stability and difficulty in recycling.
Patent Information
- Application Number
- CN202411007249.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-25
AI Technical Summary
When dealing with antibiotic pollution in water, existing zeolite-based catalysts have problems such as reduced catalytic activity, high metal ion leaching rate and secondary pollution. Moreover, their application range and stability are insufficient, making it difficult to achieve efficient and environmentally friendly antibiotic degradation.
Iron-doped ZSM5 type zeolite is used as a catalyst and prepared by hydrothermal reaction and calcination. The Fe species are evenly dispersed in the zeolite frame to form a composite morphology of nanoparticles and nanosheets, which improve catalytic activity and stabilize fixation, and use hydrogen peroxide to activate it to produce. Reactive oxygen species are degraded.
It achieves efficient degradation of antibiotics in water, has good catalyst stability, almost no Fe ions leaching, has a wide pH range, is easy to recover, has excellent degradation effect, and is suitable for large-scale applications.
Smart Images

Figure CN119034795A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment and relates to a method for degrading antibiotics in water by utilizing iron-doped ZSM5 zeolite to activate hydrogen peroxide. Background Art
[0002] More than 70% of the Earth's surface is covered by water, but the water resources available to humans are relatively scarce. This situation is partly due to the fact that humans continue to discharge pollutants into water bodies that exceed the self-purification capacity of the environment, including a considerable proportion of antibiotics. Antibiotics are widely used in the fields of human animal husbandry, health care, agriculture, etc., especially high concentrations of tetracycline pollutants discharged from veterinary sources may cause high levels of related antibiotic resistance genes (ARGs) to spread in the environment, posing a risk to human health. Therefore, the serious excess of antibiotics in the water environment, especially antibiotics represented by tetracycline, urgently requires efficient and convenient treatment processes to reduce the risk of related ARG transmission.
[0003] Advanced oxidation process (AOPs) is a chemical treatment process with the characteristics of high catalytic efficiency and environmental friendliness. Among AOPs, Fenton reaction is a representative technology with strong oxidation ability and simple operating conditions, and it performs well in treating difficult-to-degrade pollutants, especially antibiotics. However, the classic homogeneous Fenton reaction has some limitations, such as narrow reaction pH range, difficulty in catalyst separation and recovery, resulting in secondary pollution. Heterogeneous Fenton reaction can effectively solve these problems, so the selection of suitable catalysts is the key to achieving efficient degradation of antibiotics. The heterogeneous catalysts used in the Fenton technology to remove antibiotic pollutants in water bodies reported so far can be mainly divided into metal oxides, nano zero-valent metal-based catalysts, and supported catalysts. Among them, supported catalysts are relatively cheap and more convenient for large-scale application in wastewater treatment. Zeolite, as a carrier material with large cation exchange capacity, easy availability, and environmental friendliness, is widely used in advanced oxidation processes. Most importantly, zeolite can remain stable even when it comes to strong oxidizing active oxygen species such as hydroxyl radicals (·OH). However, the zeolite-based catalysts currently prepared either have the problem of reduced catalytic activity due to the agglomeration of metal species or the problem of secondary pollution caused by the leaching of metal species. It can be seen that when designing widely used zeolite-based catalysts, it is necessary to maximize the activity of metal sites and minimize the leakage of metal ions to achieve easy recycling and maintain the stability of catalytic activity. This is very important and also has important significance for promoting the practical application of zeolite-based catalysts. In addition, the use of zeolites for efficient degradation of antibiotic pollution is still in the exploratory stage, and further research and exploration of its application potential are needed. Therefore, the development of a new zeolite-based catalyst with high catalytic activity, low metal ion leaching rate, good stability and easy recovery is of great significance for efficiently activating hydrogen peroxide and efficiently degrading antibiotic pollutants in water bodies. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for degrading antibiotics in water by activating hydrogen peroxide with iron-doped ZSM5 zeolite, which has high degradation efficiency, less metal leaching, good recycling effect and is green and environmentally friendly.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite, wherein the iron-doped ZSM5 zeolite is used as a catalyst to activate hydrogen peroxide to degrade antibiotic wastewater; the iron-doped ZSM5 zeolite is prepared by sequentially mixing sodium aluminate, tetrapropylammonium hydroxide, water, tetraethoxysilane and an iron source, and undergoing hydrothermal reaction and calcination, wherein the iron source is at least one of ferrous acetylacetonate, ferric acetylacetonate or ferric nitrate.
[0007] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, and the preparation steps of the iron-doped ZSM5 zeolite include:
[0008] S1, mixing sodium aluminate, tetrapropylammonium hydroxide and water, and stirring to obtain a mixed solution A;
[0009] S2, adding tetraethoxysilane to the mixed solution A, stirring, to obtain a mixed solution B;
[0010] S3, adding an iron source to the mixed solution B, stirring, to obtain a mixed solution C;
[0011] S4, performing a hydrothermal reaction on the mixed solution C to obtain a hydrothermal reaction product;
[0012] S5. calcining the hydrothermal reaction product to obtain iron-doped ZSM5 zeolite.
[0013] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, wherein the mass ratio of tetraethoxysilane, sodium aluminate, tetrapropylammonium hydroxide, iron source and water is 8.32:0.07286:13.01:0.5:15.45.
[0014] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved. In step S4, the reaction temperature of the hydrothermal reaction is 140° C. to 190° C., and the reaction time of the hydrothermal reaction is 60 h to 108 h.
[0015] The above-mentioned method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved. In step S5, the calcination temperature is 500°C to 650°C, the calcination heating rate is 1°C / min to 6°C / min, and the calcination time is 2h to 7h.
[0016] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved in that in step S1, the stirring time is 1 hour to 4 hours.
[0017] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved in that in step S2, the stirring time is 4h to 7h.
[0018] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved in that in step S3, the stirring time is 1 hour to 4 hours.
[0019] The above-mentioned method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, and the following treatments are included after the hydrothermal reaction: washing and drying the reaction product; the washing is performed by washing with water 4 to 9 times, the drying temperature is 60°C to 110°C, and the drying time is 8h to 16h.
[0020] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, wherein the degradation treatment is: mixing the iron-doped ZSM5 zeolite with antibiotic wastewater, adding hydrogen peroxide solution, and performing a catalytic degradation reaction.
[0021] The above-mentioned method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, wherein the concentration of hydrogen peroxide in the antibiotic wastewater is 5mmol / L~40mmol / L, the concentration of iron-doped ZSM5 zeolite in the antibiotic wastewater is 0.1g / L~0.4g / L; the initial concentration of antibiotics in the antibiotic wastewater is ≤10mg / L; and the initial concentration of the hydrogen peroxide solution is 1mol / L.
[0022] The above method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, wherein the antibiotic in the antibiotic wastewater is at least one of tetracycline hydrochloride, norfloxacin, and sulfamethoxazole.
[0023] The above-mentioned method of using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water is further improved, wherein the mixing process of the iron-doped ZSM5 zeolite and antibiotic wastewater is carried out under stirring conditions, the stirring speed is 250r / min~500r / min, the stirring time is 25min~60min, the catalytic degradation reaction time is 30min~60min, and the catalytic degradation reaction temperature is 288.15K~313.15K.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] (1) The present invention provides a method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite, wherein the antibiotic pollutants in the water are treated by activating hydrogen peroxide using iron-doped ZSM5 zeolite as a catalyst, wherein the iron-doped ZSM5 zeolite is prepared by sequentially mixing sodium aluminate, tetrapropylammonium hydroxide, water, urea, tetraethoxysilane, and an iron source, and undergoing a hydrothermal reaction and calcination, and the iron source is at least one of ferrous acetylacetonate, ferric acetylacetonate, or ferric nitrate. In the present invention, sodium aluminate, tetrapropylammonium hydroxide, water, urea, tetraethoxysilane and an iron source are used as raw materials, wherein the iron source is at least one of ferrous acetylacetonate, ferric acetylacetonate or ferric nitrate. Fe species are first doped into the ZSM5 zeolite framework by a hydrothermal synthesis method, and then the Fe species are uniformly dispersed and stably fixed in the zeolite framework during the calcination process. On the one hand, the prepared iron-doped ZSM5 zeolite has a composite morphology of nanoparticles and nanosheets, has the advantages of large specific surface area and strong adsorption capacity, which is conducive to the rapid adsorption of antibiotics in wastewater by the iron-doped ZSM5 zeolite. On the other hand, the Fe species are uniformly dispersed in the zeolite framework, which can not only increase the number of catalytic active sites, but also increase the contact probability of the active sites with pollutants, showing very excellent catalytic activity, thereby achieving efficient activation of hydrogen peroxide (H2O2) to produce ·OH and superoxide free radicals ·O2 - and singlet oxygen 1O2 and other active oxygen species, and then use these active oxygen species to efficiently degrade antibiotics in water. More importantly, by stably fixing Fe species in the zeolite framework, the stability of Fe species can be significantly improved, making it difficult to leach, not only can it be reused to treat antibiotic wastewater, but also can achieve Fe ion leaching of 0mg / L in the entire degradation process, without causing secondary pollution to the environment. Taking tetracycline hydrochloride (TC) as an example, the iron-doped ZSM5 zeolite prepared by the hydrothermal method adopted in the inventive method can completely remove tetracycline hydrochloride in wastewater within 40min, and the removal rate reaches 100%, while under the same conditions, the iron-doped ZSM5 zeolite prepared by the conventional impregnation method and ion exchange method has a removal rate of 29.6% and 17.3% higher than that of tetracycline hydrochloride, respectively. At the same time, in the cycle test, the iron-doped ZSM5 zeolite has no obvious deactivation and still maintains a high catalytic activity. After five cycle experiments, the removal rate of TC is still 100.0%. In addition, it exhibits obvious magnetism before and after use, indicating that it can be easily recovered through a magnetic field, thereby preventing the catalyst from being present in a water environment for a long time and possibly causing secondary pollution. In addition, the method of the present invention also expands the applicable pH range of the treatment of antibiotic pollutants in water bodies by iron-doped ZSM5 zeolite. The process has a good oxidation removal effect on antibiotics in water bodies within the initial pH range of 3.0 to 9.0. Even under the condition of pH 8.99, a removal effect of nearly 80% of tetracycline was achieved within 60 minutes of the experiment, overcoming the defect that some Fenton reactions must require acidic pH for the system. In addition, the method of the present invention exhibits good adsorption and oxidation degradation capabilities for different types of antibiotics, and has high practicality. Therefore, in the present invention, the iron-doped ZSM5 zeolite used has the advantages of uniformly dispersed active sites, high catalytic activity, good stability, strong magnetism and easy recovery. When used for activating hydrogen peroxide, a large number of active oxygen species can be generated, and then these active oxygen species can be used to achieve efficient degradation of antibiotics in wastewater. In particular, during use, Fe species are almost not leached, and it has the advantages of good degradation effect, green environmental protection, wide pH application range, magnetic recovery, good reusability, convenient operation, low cost, etc., and can achieve efficient degradation of different types of antibiotic wastewater, and has high use value and good application prospects.
[0026] (2) The method of the present invention can perform well in degrading antibiotic pollution, is simple and easy to operate, and has the characteristics of low cost, environmental friendliness, and easy recovery of catalysts. It is suitable for promotion and can efficiently remove antibiotic pollutants in water bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0028] Figure 1 XRD diagrams of the iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe(III)@ZSM5) prepared in Examples 1 and 2 of the present invention, the iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IM) prepared by the wet impregnation method in Comparative Example 1, and the iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IE) prepared by the ion exchange method in Comparative Example 2.
[0029] Figure 2 This is a SEM image of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1 of the present invention.
[0030] Figure 3 This is a TEM image of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1 of the present invention.
[0031] Figure 4 This is a comparison chart of the degradation effects of iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe(III)@ZSM5) prepared in Examples 1 and 2 of the present invention, iron-doped ZSM5 zeolites prepared by wet impregnation method in Comparative Example 1 (Fe(III) / ZSM5-IM), and iron-doped ZSM5 zeolites prepared by ion exchange method in Comparative Example 2 (Fe(III) / ZSM5-IE) on tetracycline hydrochloride in water.
[0032] Figure 5 This is a graph showing the degradation effect of different antibiotics on hydrogen peroxide activated by iron-doped ZSM5 zeolite (Fe(II)@ZSM5, Fe-N@ZSM5) in Examples 3 and 4 of the present invention.
[0033] Figure 6 This is a diagram showing the degradation effect of tetracycline hydrochloride on iron-doped ZSM5 zeolite (Fe(II)@ZSM5) activated with hydrogen peroxide under different pH conditions in Example 5 of the present invention.
[0034] Figure 7 This is a diagram showing the degradation effect of tetracycline hydrochloride in water by the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) of Example 7 of the present invention in a recycling experiment.
[0035] Figure 8 This is the hysteresis loop diagram of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) before and after use in Example 7 of the present invention. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0037] In the following examples of the present invention, unless otherwise specified, the materials and instruments used are commercially available, the equipment used is conventional equipment, and the data obtained are the average values of more than three repeated experiments.
[0038] Example 1
[0039] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite, specifically using iron-doped ZSM5 zeolite and hydrogen peroxide to degrade tetracycline hydrochloride wastewater, comprising the following steps:
[0040] 15 mg of iron-doped ZSM5 zeolite (Fe(II)@ZSM5) was weighed and added to 50 mL of a 10 mg / L, pH=4.4 tetracycline hydrochloride solution. The solution was magnetically stirred at a speed of 450 r / min for 30 min to reach adsorption equilibrium. A 1 mol / L hydrogen peroxide solution was added to make the hydrogen peroxide concentration in the system 20 mM. The catalytic degradation reaction was carried out at a temperature of 298.15 K for 60 min to complete the degradation of tetracycline hydrochloride in the water.
[0041] In this embodiment, the preparation method of iron-doped ZSM5 zeolite (Fe(II)@ZSM5) comprises the following steps:
[0042] (1) Add 0.07286 g of sodium aluminate, 13.01 g of tetrapropylammonium hydroxide and 15.45 g of water into a beaker and stir for 2 h to obtain a mixed solution A.
[0043] (2) 8.32 g of tetraethoxysilane was gradually added to the mixed solution A obtained in step (1) within 30 seconds, and the mixture was stirred for 6 hours and mixed evenly to obtain a mixed solution B.
[0044] (3) Add 0.5 g of ferrous acetylacetonate to the mixed solution B obtained in step (2), stir for 2 h, and mix evenly to obtain a mixed solution C.
[0045] (4) The mixed solution C obtained in step (3) is subjected to a hydrothermal reaction. The hydrothermal reaction is carried out in a high-pressure reactor at a temperature of 170° C. for 70 h. After completion, the mixture is taken out and cooled. The reaction product is washed 7 times with ultrapure water and then dried in an electric blast drying oven at 105° C. for 10 h.
[0046] (5) The dried product in step (4) is placed in a muffle furnace for calcination at a temperature of 550° C., a heating rate of 2° C. / min, and a calcination time of 6 h to obtain an iron-doped ZSM5 zeolite, denoted as Fe(II)@ZSM5.
[0047] Embodiment 2:
[0048] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite is basically the same as the method in Example 1, except that the catalyst used is iron-doped ZSM5 zeolite (Fe(III)@ZSM5) prepared using ferric acetylacetonate as an iron source.
[0049] In this embodiment, the preparation method of iron-doped ZSM5 zeolite (Fe(III)@ZSM5) comprises the following steps:
[0050] (1) Add 0.07286 g of sodium aluminate, 13.01 g of tetrapropylammonium hydroxide and 15.45 g of water into a beaker and stir for 2 h to obtain a mixed solution A.
[0051] (2) 8.32 g of tetraethoxysilane was gradually added to the mixed solution A obtained in step (1) within 30 seconds, and the mixture was stirred for 6 hours and mixed evenly to obtain a mixed solution B.
[0052] (3) Add 0.5 g of ferric acetylacetonate to the mixed solution B obtained in step (2), stir for 2 h, and mix evenly to obtain a mixed solution C.
[0053] (4) The mixed solution C obtained in step (3) is subjected to a hydrothermal reaction. The hydrothermal reaction is carried out in a high-pressure reactor at a temperature of 170° C. for 70 h. After completion, the mixture is taken out and cooled. The reaction product is washed 7 times with ultrapure water and then dried in an electric blast drying oven at 105° C. for 10 h.
[0054] (5) The dried product in step (4) is placed in a muffle furnace for calcination at a temperature of 550° C., a heating rate of 2° C. / min, and a calcination time of 6 h to obtain an iron-doped ZSM5 zeolite, denoted as Fe(III)@ZSM5.
[0055] Comparative Example 1:
[0056] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite is basically the same as the method in Example 1, except that the catalyst used is iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IM) prepared by wet impregnation method.
[0057] In this embodiment, the method for preparing iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IM) by wet impregnation method comprises the following steps:
[0058] (1) First, 0.07 g of iron acetylacetonate and 2 g of ZSM5 zeolite (commercially available) were suspended in 120 mL of ultrapure water and mechanically stirred at 40° C. until the water evaporated to obtain a solid.
[0059] (2) Dry the solid obtained in step (1) in an electric heated air drying oven at 105° C. for 10 h.
[0060] (3) The dried product in step (2) is placed in a muffle furnace for calcination at a temperature of 550° C., a heating rate of 2° C. / min, and a calcination time of 6 h to obtain an iron-doped ZSM5 zeolite prepared by a wet impregnation method, which is recorded as Fe(III) / ZSM5-IM.
[0061] Comparative Example 2:
[0062] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite is basically the same as the method in Example 1, except that the catalyst used is iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IE) prepared by ion exchange method.
[0063] In this embodiment, the preparation method of iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IE) prepared by ion exchange method comprises the following steps:
[0064] (1) First, 0.07 g of iron acetylacetonate and 2 g of ZSM5 zeolite (commercially available) were suspended in 120 mL of ultrapure water and mechanically stirred at room temperature for 1 day.
[0065] (2) The solid obtained in step (1) was centrifugally washed with ultrapure water for more than two times to remove excess iron species that did not participate in ion exchange, and then dried in an electric heated blast drying oven at 105° C. for 10 h.
[0066] (3) The dried product in step (2) is placed in a muffle furnace for calcination at a temperature of 550° C., a heating rate of 2° C. / min, and a calcination time of 6 h to obtain an iron-doped ZSM5 zeolite prepared by an ion exchange method, which is recorded as Fe(III) / ZSM5-IE.
[0067] Figure 1The XRD patterns of the iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe(III)@ZSM5) prepared in Examples 1 and 2 of the present invention, the iron-doped ZSM5 zeolites (Fe(III) / ZSM5-IM) prepared by the wet impregnation method in Comparative Example 1, and the iron-doped ZSM5 zeolites (Fe(III) / ZSM5-IE) prepared by the ion exchange method in Comparative Example 2 are shown in FIG. Figure 1 It can be seen that after comparing the four zeolite-based catalysts, Fe(II)@ZSM5, Fe(III)@ZSM5, Fe(III) / ZSM5-IM and Fe(III) / ZSM5-IE, with the PDF standard card of ZSM5 zeolite, they all conform to the characteristic peaks of typical ZSM5 zeolite and are consistent with the crystal structure of zeolite.
[0068] Figure 2 This is a SEM image of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1 of the present invention. Figure 2 In the figure, (a) is the 100nm ruler, and (b) is the 200nm ruler. Figure 2 It can be seen that Fe(II)@ZSM5 presents a uniform composite structure of nanoparticles and nanosheets with a large specific surface area, indicating that it has good adsorption capacity. At the same time, there are no obvious iron oxide particles, indicating that the Fe species are uniformly dispersed and the catalyst has good catalytic activity.
[0069] Figure 3 This is a TEM image of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1 of the present invention. Figure 3 In the figure, (a) is a 20nm ruler, and (b) is a 200nm ruler. Figure 3 It can be seen that under the condition that the scale of (a) is 20nm, there are obvious lattice fringes, and the lattice spacing is 0.98nm, which is basically consistent with the (0 20) crystal plane in the standard card PDF#44-0003 of ZSM5, which once again confirms that it maintains the crystal structure of ZSM5. Figure 3 It can be seen that in (b) the scale is 200 nm and the corresponding X-ray energy spectrum elemental image analysis technology (EDS mapping), the uniform distribution of Fe element is directly confirmed.
[0070] During the magnetic stirring and degradation process of Example 1-2 and Comparative Example 1-2, 1 mL of sample was taken every 10 min, and the sample was filtered with a 0.22 μm filter head. The filtrate was measured by liquid chromatography to determine the concentration of pollutants after adsorption and degradation, thereby obtaining the adsorption effect and catalytic degradation effect of different types of iron-doped ZSM5 zeolites on antibiotics. The results are shown in FIG. Figure 4 shown.
[0071] Figure 4The figure is a comparison of the degradation effects of the iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe(III)@ZSM5) prepared in Examples 1 and 2 of the present invention, the iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IM) prepared by the wet impregnation method in Comparative Example 1, and the iron-doped ZSM5 zeolite (Fe(III) / ZSM5-IE) prepared by the ion exchange method in Comparative Example 2 on tetracycline hydrochloride in water. Figure 4 It can be seen that after 30 minutes of adsorption and 40 minutes of oxidative degradation, the removal rates of tetracycline hydrochloride by Fe(II)@ZSM5, Fe(III)@ZSM5, Fe(III) / ZSM5-IM, and Fe(III) / ZSM5-IE through activation of hydrogen peroxide H2O2 were 100%, 99.9%, 70.4%, and 82.7%, respectively. This is because the Fe(II)@ZSM5 prepared by ferrous acetylacetonate as an iron source has higher catalytic activity and is easier to undergo Fenton reaction with H2O2. At the same time, it can be seen that the catalytic performance of the iron-doped ZSM5 zeolite prepared by the hydrothermal synthesis method is significantly better than that of the zeolite-based catalyst prepared by the wet impregnation method or ion exchange method. This indicates that due to the excellent stability of the organic iron precursor under alkaline conditions, the Fe species may be doped into the zeolite framework in the form of a complex during the hydrothermal synthesis process, thereby obtaining a more uniform morphology and higher activity, which is conducive to the activation of hydrogen peroxide to produce ·OH, ·O2 - and 1 O2 and other reactive oxygen species, thereby efficiently degrading antibiotics.
[0072] Embodiment 3:
[0073] A method for degrading antibiotics in water by using iron-doped ZSM5 zeolite to activate hydrogen peroxide, specifically using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade tetracycline hydrochloride, sulfamethoxazole, and norfloxacin wastewater, respectively, comprising the following steps:
[0074] Weigh 3 portions of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1, 15 mg each, and add them to a tetracycline hydrochloride (TC) solution, a sulfamethoxazole (SMX) solution, and a norfloxacin (NOR) solution, respectively. The volume of each solution is 50 mL and the concentration is 10 mg / L. The mixture is stirred magnetically at a speed of 450 r / min for 30 min to reach adsorption equilibrium. A hydrogen peroxide solution with a concentration of 1 mol / L is added to make the hydrogen peroxide concentration in the system 20 mM. The degradation reaction is carried out at a temperature of 298.15 K for 60 min to complete the degradation of various antibiotics in the water.
[0075] During the magnetic stirring and degradation process, 1 mL of sample was taken every 10 minutes, and the sample was filtered with a 0.22 μm filter head. The filtrate was measured by liquid chromatography to determine the pollutant concentration after adsorption and degradation, thereby obtaining the adsorption effect and catalytic degradation effect of the iron-doped ZSM5 zeolite of the present invention on various antibiotics.
[0076] Embodiment 4:
[0077] A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite, specifically utilizing iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade tetracycline hydrochloride, sulfamethoxazole, and norfloxacin wastewater, which is basically the same as the method in Example 3, except that the catalyst used is iron-doped ZSM5 zeolite (Fe-N@ZSM5) prepared by using ferric nitrate nonahydrate as an iron source.
[0078] In this embodiment, the preparation method of iron-doped ZSM5 zeolite (Fe-N@ZSM5) comprises the following steps:
[0079] (1) Add 0.07286 g of sodium aluminate, 13.01 g of tetrapropylammonium hydroxide and 15.45 g of water into a beaker and stir for 2 h to obtain a mixed solution A.
[0080] (2) 8.32 g of tetraethoxysilane was gradually added to the mixed solution A obtained in step (1) within 30 seconds, and the mixture was stirred for 6 hours and mixed evenly to obtain a mixed solution B.
[0081] (3) Add 0.5 g of ferric nitrate nonahydrate to the mixed solution B obtained in step (2), stir for 2 h, and mix well to obtain a mixed solution C;
[0082] (4) The mixed solution C obtained in step (3) is subjected to a hydrothermal reaction. The hydrothermal reaction is carried out in a high-pressure reactor at a temperature of 170° C. for 70 h. After completion, the mixture is taken out and cooled. The reaction product is washed 7 times with ultrapure water and then dried in an electric blast drying oven at 105° C. for 10 h.
[0083] (5) The dried product in step (4) is placed in a muffle furnace for calcination at a temperature of 550° C., a heating rate of 2° C. / min, and a calcination time of 6 h to obtain an iron-doped ZSM5 zeolite, denoted as Fe-N@ZSM5.
[0084] During the magnetic stirring and degradation process, 1 mL of sample was taken every 10 minutes, and the sample was filtered with a 0.22 μm filter head. The filtrate was measured by liquid chromatography to determine the pollutant concentration after adsorption and degradation, thereby obtaining the adsorption effect and catalytic degradation effect of the iron-doped ZSM5 zeolite of the present invention on various antibiotics.
[0085] Figure 5 The figure shows the degradation effect of different antibiotics on hydrogen peroxide activated by iron-doped ZSM5 zeolite (Fe(II)@ZSM5, Fe-N@ZSM5) in Examples 3 and 4 of the present invention. Figure 5 It can be seen that when the degradation reaction lasts for 60 minutes, the removal rates of Fe(II)@ZSM5 for tetracycline hydrochloride (TC) solution, sulfamethoxazole (SMX) solution, and norfloxacin (NOR) solution reach 100%, 89.5%, and 100%, respectively, and the removal rates of Fe-N@ZSM5 for tetracycline hydrochloride (TC) solution, sulfamethoxazole (SMX) solution, and norfloxacin (NOR) solution all reach 100%. It can be seen that the iron-doped ZSM5 zeolite (Fe(II)@ZSM5, Fe-N@ZSM5) activated by hydrogen peroxide prepared with ferric acetylacetonate and ferric nitrate nonahydrate as the iron source of the present invention shows excellent degradation effect on various antibiotics.
[0086] Embodiment 5:
[0087] A method for degrading antibiotics in water by using iron-doped ZSM5 zeolite to activate hydrogen peroxide, specifically using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade tetracycline hydrochloride wastewater with different pH values, comprising the following steps:
[0088] Weigh 4 portions of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1, 15 mg each, and add them to tetracycline hydrochloride solutions with pH values of 3.02, 4.99, 7.07, and 8.99, respectively. The volume of each solution is 50 mL, the concentration is 10 mg / L, and magnetic stirring is performed at a speed of 450 r / min for 30 min to reach adsorption equilibrium, and then a hydrogen peroxide solution with a concentration of 1 mol / L is added to make the hydrogen peroxide concentration in the system 20 mM. The degradation reaction is carried out at a temperature of 298.15 K for 60 min to complete the degradation of tetracycline hydrochloride in the water.
[0089] During the magnetic stirring and degradation process, 1 mL of sample was taken every 10 minutes and filtered with a 0.22 μm filter head. The filtrate was measured by liquid chromatography to determine the pollutant concentration after adsorption and degradation, thereby obtaining the adsorption effect and catalytic degradation effect of iron-doped ZSM5 zeolite on tetracycline hydrochloride under different pH conditions.
[0090] Figure 6 The figure is a graph showing the degradation effect of tetracycline hydrochloride on the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) activated by hydrogen peroxide under different pH conditions in Example 5 of the present invention. Figure 6It can be seen that the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) of the present invention has a removal rate of 100% for tetracycline hydrochloride under acidic and neutral pH conditions, and also achieves a removal effect of more than 80% under alkaline pH conditions, indicating that the method of the present invention has a wide pH application range and can overcome the disadvantage that some Fenton reactions must require acidic pH for the system.
[0091] Embodiment 6:
[0092] The leaching of Fe from iron-doped ZSM5 zeolite during the degradation of TC and SMX was investigated.
[0093] The iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe-N@ZSM5) prepared in Example 1 and Example 4 were respectively used to activate hydrogen peroxide to degrade TC and SMX in water, which was basically the same as Example 1, except that the solutions of TC and SMX were subjected to magnetic stirring and degradation, and 2 mL of sample was taken after 90 min of co-reaction, and the sample was filtered with a 0.22 μm filter head, and 1 mL of filtrate was taken in a 10 mL centrifuge tube, and 4 mL of ultrapure water was added. After mixing, the concentration of Fe ions leached during the reaction was determined by inductively coupled plasma mass spectrometry, and the results are shown in Table 1.
[0094] Table 1 Comparison of Fe leaching concentrations of iron-doped ZSM5 zeolites (Fe(II)@ZSM5, Fe-N@ZSM5) prepared in Example 1 and Example 4 during activation of hydrogen peroxide to degrade antibiotic wastewater
[0095] Catalyst type Types of antibiotics Reaction time (min) Fe ion leaching concentration (mg / L) Fe(II)@ZSM5 Tetracycline Hydrochloride(TC) 90 0 Fe(II)@ZSM5 Sulfamethoxazole (SMX) 90 0 Fe-N@ZSM5 Tetracycline Hydrochloride(TC) 90 0 Fe-N@ZSM5 Sulfamethoxazole (SMX) 90 0
[0096] As can be seen from Table 1, the iron-doped ZSM5 zeolite (Fe(II)@ZSM5, Fe-N@ZSM5) of the present invention leached 0 mg / L of Fe during the process of activating hydrogen peroxide to degrade antibiotics. It can be seen that the preparation method of the present invention can make the Fe species very stably doped in the zeolite framework, and almost no Fe is leached during the degradation process, thereby better avoiding secondary pollution.
[0097] Embodiment 7:
[0098] The repeated degradation effect of the iron-doped ZSM5 zeolite was investigated. Specifically, the iron-doped ZSM5 zeolite prepared in Example 1 was used to activate hydrogen peroxide to degrade tetracycline hydrochloride wastewater, and the catalyst was recovered to degrade new tetracycline hydrochloride wastewater, comprising the following steps:
[0099] (1) 15 mg of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) prepared in Example 1 was weighed and added to a tetracycline hydrochloride solution with a volume of 50 mL, a concentration of 10 mg / L, and a pH of 4.4. The solution was stirred magnetically at a speed of 450 r / min for 30 min to reach adsorption equilibrium. A hydrogen peroxide solution with a concentration of 1 mol / L was added to make the hydrogen peroxide concentration in the system 20 mM. The degradation reaction was carried out at a temperature of 298.15 K for 60 min to complete the degradation of tetracycline hydrochloride in the water.
[0100] (2) After the degradation is completed, the catalyst is washed with water three times and ethanol three times, and dried in an electric heated forced air drying oven at 105° C. for 10 h to complete the operation of recovering the catalyst.
[0101] (3) Repeat the operations in steps (1) and (2) to adsorb and degrade the new tetracycline hydrochloride solution, and repeat this process 5 times in total.
[0102] During the magnetic stirring and degradation process, 1 mL of sample is taken every 10 minutes, and the sample is filtered with a 0.22 μm filter head. The filtrate is measured by liquid chromatography to determine the pollutant concentration after adsorption and after degradation, thereby obtaining the adsorption effect and catalytic degradation effect of the iron-doped ZSM5 zeolite of the present invention on tetracycline hydrochloride in water in a recycling recovery experiment.
[0103] Figure 7 This is a graph showing the degradation effect of iron-doped ZSM5 zeolite (Fe(II)@ZSM5) on tetracycline hydrochloride in water in a recycling experiment in Example 7 of the present invention. Figure 7 It can be seen that in the 5-cycle experiment, the catalytic activity of Fe(II)@ZSM5 did not decrease significantly, and the removal rate of tetracycline hydrochloride could still reach 100%, showing good stability.
[0104] Figure 8 : This is a hysteresis loop diagram of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) before and after use in Example 7 of the present invention. Figure 8 It can be seen that the hysteresis loops of the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) before use and the iron-doped ZSM5 zeolite (Fe(II)@ZSM5) recovered after five cycles both exhibit ferromagnetism / ferrimagnetism, with saturation magnetization intensities of 0.653emu / g and 0.632emu / g, respectively, confirming that the materials are strong magnetic materials that can be effortlessly recovered through a magnetic field after use, thereby preventing secondary pollution that may be caused by the long-term presence of the catalyst in an aqueous environment.
[0105] From the above results, it can be seen that in the present invention, the iron-doped ZSM5 zeolite used has the advantages of uniform dispersion of active sites, high catalytic activity, good stability, strong magnetism and easy recovery. When used to activate hydrogen peroxide, a large amount of active oxygen species can be generated, and then these active oxygen species can be used to achieve efficient degradation of antibiotics in wastewater. In particular, during use, Fe species are almost not leached. Therefore, the method of the present invention using iron-doped ZSM5 zeolite to activate hydrogen peroxide to degrade antibiotics in water can achieve efficient degradation of different types of antibiotic wastewater, has the advantages of good degradation effect, green environmental protection, wide pH application range, magnetic recovery, good reusability, convenient operation, low cost, etc., is a new method suitable for popularization and application and can efficiently and thoroughly remove antibiotic pollution in water, has high use value and good application prospects.
[0106] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite, characterized in that: The antibiotic wastewater is degraded by using iron-doped ZSM5 zeolite as a catalyst to activate hydrogen peroxide; the iron-doped ZSM5 zeolite is prepared by sequentially mixing sodium aluminate, tetrapropylammonium hydroxide, water, tetraethoxysilane and an iron source, and then undergoing hydrothermal reaction and calcination; the iron source is at least one of ferrous acetylacetonate, ferric acetylacetonate or ferric nitrate.
2. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 1, characterized in that: The preparation steps of the iron-doped ZSM5 zeolite include: S1, mixing sodium aluminate, tetrapropylammonium hydroxide and water, and stirring to obtain a mixed solution A; S2, adding tetraethoxysilane to the mixed solution A, stirring, to obtain a mixed solution B; S3, adding an iron source to the mixed solution B, stirring, to obtain a mixed solution C; S4, performing a hydrothermal reaction on the mixed solution C to obtain a hydrothermal reaction product; S5. calcining the hydrothermal reaction product to obtain iron-doped ZSM5 zeolite.
3. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 2, characterized in that: The mass ratio of the tetraethoxysilane, sodium aluminate, tetrapropylammonium hydroxide, iron source and water is 8.32:0.07286:13.01:0.5:15.
45.
4. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 2, characterized in that: In step S4, the reaction temperature of the hydrothermal reaction is 140° C. to 190° C., and the reaction time of the hydrothermal reaction is 60 h to 108 h; In step S5, the calcination temperature is 500°C to 650°C, the calcination heating rate is 1°C / min to 6°C / min, and the calcination time is 2h to 7h.
5. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 2, characterized in that: In step S1, the stirring time is 1 h to 4 h; In step S2, the stirring time is 4h to 7h; In step S3, the stirring time is 1 h to 4 h.
6. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 2, characterized in that: The following treatments are included after the hydrothermal reaction: washing and drying the reaction product; the washing is performed with water for 4 to 9 times, the drying temperature is 60° C. to 110° C., and the drying time is 8 hours to 16 hours.
7. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to any one of claims 1 to 6, characterized in that: The degradation treatment comprises: mixing iron-doped ZSM5 zeolite with antibiotic wastewater, adding hydrogen peroxide solution, and performing catalytic degradation reaction.
8. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 7, characterized in that: The concentration of hydrogen peroxide in the antibiotic wastewater is 5mmol / L to 40mmol / L, the concentration of iron-doped ZSM5 zeolite in the antibiotic wastewater is 0.1g / L to 0.4g / L; the initial concentration of antibiotics in the antibiotic wastewater is ≤10mg / L; and the initial concentration of the hydrogen peroxide solution is 1mol / L.
9. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 8, characterized in that: The antibiotic in the antibiotic wastewater is at least one of tetracycline hydrochloride, norfloxacin and sulfamethoxazole.
10. The method for degrading antibiotics in water by activating hydrogen peroxide using iron-doped ZSM5 zeolite according to claim 9, characterized in that: The mixing process of the iron-doped ZSM5 zeolite and antibiotic wastewater is carried out under stirring conditions, the stirring speed is 250r / min~500r / min, the stirring time is 25min~60min, the catalytic degradation reaction time is 30min~60min, and the catalytic degradation reaction temperature is 288.15K~313.15K.
Citation Information
Patent Citations
Method for preparing microporous-mesoporous composite Fe-ZSM-5 zeolite molecular sieve catalyst
CN102125868A
Fe-ZSM-5 catalyst used in NOx selective catalytic reduction, and preparation method thereof
CN103386322A
Treatment method of wastewater containing xanthate
CN108706771A
Preparation method of Fe-HZSM-5 heteroatom molecular sieve
CN111229301A
Fe-ZSM-5 molecular sieve catalyst with high Fe species dispersibility and preparation method thereof
CN117244586A
Cited By
Method for hydrothermally synthesizing iron-doped skeleton hollow molecular sieve material by utilizing ion exchange to assist and application of iron-doped skeleton hollow molecular sieve material