Full-biodegradable ultrahigh-barrier reinforced paper and preparation method thereof
By using NMMO dissolved regenerated cellulose technology and cationically modified microfibrillated cellulose on paper-based materials, an ultra-thin dense layer is formed, which solves the problem of insufficient barrier performance of paper-based materials and achieves ultra-high barriers that are fully biodegradable Reinforced paper, excellent barrier and mechanical properties, and simplifies the preparation process.
Patent Information
- Application Number
- CN202411052272.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
Due to the hydrophilic behavior and porous structure of paper-based packaging materials, they cannot effectively block gas and water vapor, resulting in limited application in the packaging field. The existing high-barrier materials are made in complex or contain non-degradable ingredients, and can be fully biodegradable. Inadequate barrier performance.
Using N-methylmorpholine-N-oxide (NMMO) aqueous solution to dissolve regenerated cellulose technology, an ultra-thin dense regenerated cellulose film is formed on the surface of the base paper, combined with cationically modified microfibrillated cellulose, strengthening the paper-based material Mechanical and barrier properties.
It realizes fully biodegradable ultra-high barrier reinforcement paper, with excellent water vapor barrier, oxygen barrier, mechanical strength and low water absorption, simplifies the preparation process, avoids high temperature and high pressure operation, and is environmentally friendly and safe.
Smart Images

Figure CN118958046A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of paper-based packaging materials, relates to a fully biodegradable ultra-high barrier reinforced paper and a preparation method thereof, and particularly relates to a method for applying dissolving pulp regenerated cellulose to paper-based barrier packaging materials. Background Art
[0002] Paper-based barrier packaging materials have great application potential in the packaging field because of their excellent advantages such as being eco-friendly, renewable and biodegradable. However, the hydrophilic behavior and porous structure of paper-based materials hinder the widespread application of paper-based packaging. Compared with plastic packaging, paper-based materials have more pores, providing diffusion and mass transfer pathways for gases such as air, oxygen and water vapor. In addition, paper fibers contain rich hydroxyl structures, which make them highly hydrophilic, so they are usually not directly used in the packaging field.
[0003] To overcome this problem, paper-based materials are often combined with other materials, such as plastic or aluminum foil, to improve barrier properties at the expense of their environmental friendliness and biodegradability. There is an urgent need for greener, more environmentally friendly and safer methods to address the related defects of paper-based materials in the packaging field.
[0004] In recent years, domestic and foreign researchers have actively carried out some research work in the field of paper-based packaging to replace aluminum-plastic composites. For example, patent CN 117364541 A discloses a biodegradable high barrier (water, oil, oxygen, water vapor) paper-based packaging material and its preparation method. From bottom to top, five layers are arranged in sequence, including a base paper layer, a starch layer, a polyethylene layer, a polyepoxy oil resin layer and a polyacrylic acid resin layer, so as to achieve good moisture barrier, oxygen barrier, waterproof and oil-proof functions. Patent CN115976882 B discloses a high barrier organic-inorganic paper-based composite material and its preparation method. The composite material is obtained by sequentially coating a first organic barrier layer (degradable polymer dispersion), an inorganic barrier layer (polydopamine-modified inorganic nanomaterial), and a second organic barrier layer (degradable waterproof and oil-proof polymer dispersion) on base paper. The composite material with the above structure is based on the crosslinking and hydrolysis of polydopamine and aminosilane coupling agent to tightly connect the inorganic materials to form a dense layer, and combined with organic biomass materials to solve the barrier problem of paper-based materials. Patent CN 115573190 B discloses a method for preparing a reactive self-crosslinking polyvinyl alcohol (PVA) high barrier paper-based material. The high barrier paper-based material is prepared by preparing a polyvinyl alcohol (PVA) casting solution with persulfate and cellulose microfibrils (CNF), then spin coating and drying on the paper base.
[0005] Some of the currently disclosed paper-based materials with high barrier properties have complex preparation processes, often requiring multi-layer composites, or adding some non-degradable organic components or high-cost additives. Some fully biodegradable ones often have insufficient barrier properties and mechanical properties. Summary of the invention
[0006] In view of the defects and shortcomings of the prior art, the present invention provides a fully biodegradable ultra-high barrier reinforced paper. On the one hand, the reinforced paper utilizes the good solubility of natural cellulose fiber in N-methylmorpholine-N-oxide (NMMO) aqueous solution to prepare a uniform and stable NMMO / cellulose / water solution as a coating modification liquid. On the other hand, the dissolution-regeneration behavior of dissolving pulp cellulose fiber in NMMO aqueous solution under certain conditions is utilized to form an ultra-thin and dense regenerated cellulose film on the surface of the base paper composed of natural cellulose fiber, so as to give the base paper with different physical and chemical properties good barrier properties and mechanical properties, thereby obtaining a fully biodegradable ultra-high barrier reinforced paper. In addition, another object of the present invention is to provide a method for preparing the fully biodegradable ultra-high barrier reinforced paper.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A fully biodegradable ultra-high barrier reinforced paper, comprising a base paper layer and a regenerated cellulose layer; the regenerated fiber layers are arranged on the front and back sides of the base paper layer respectively. The base paper layer comprises one or more conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood wood pulp, bamboo pulp, bagasse pulp, and a special fiber that has been subjected to physical and chemical treatment - cationic modified microfibrillated cellulose; the regenerated fiber layer comprises regenerated cellulose fibers.
[0009] The present invention utilizes cationic modified microfibrillated cellulose that is homologous to natural pulp fibers as a reinforcing agent for the base paper layer. Conventional pulp fibers are rich in hydroxyl groups on the surface, and the carboxyl groups introduced during the pulping process make the surface of conventional pulp fibers negatively charged. The present invention innovatively selects microfibrillated cellulose modified with quaternary ammonium salts. On the one hand, it utilizes the higher specific surface area and higher aspect ratio of microfibrillated cellulose, and utilizes the physical interweaving and entanglement effect to increase the bonding area between pulp fibers; on the other hand, the microfibrillated cellulose modified with quaternary ammonium salts contains a certain amount of amino groups so that the surface is positively charged, and the bonding force with conventional pulp fibers can be increased through electrostatic adsorption. Through the above two forms of action, the addition of cationic modified microfibrillated cellulose significantly improves the mechanical strength performance of the base paper layer.
[0010] The present invention utilizes the difference in solubility of natural cellulose in NMMO / water solutions of different concentrations, and adopts a traditional coating method to form an ultra-thin regenerated cellulose film with a dense physical structure on the surface of the base paper layer. Due to the intramolecular and intermolecular hydrogen bonding force and the highly crystalline regular structure of natural cellulose fibers, the melting point of cellulose fibers is higher than the decomposition temperature, which limits their reprocessing by melting, and also makes cellulose fibers difficult to dissolve in conventional solvents. In the 1990s, a method and technology for preparing regenerated cellulose fibers using an aqueous solution of N-methylmorpholine-N-oxide (NMMO) as a solvent was developed. Compared with other solvents, NMMO aqueous solutions are non-toxic and harmless, and have a high recycling rate. The dissolution of natural cellulose fiber in high concentration NMMO / water solution (concentration above 70%) is a physical process. NMMO small molecules enter the amorphous region and crystalline region of cellulose macromolecules in turn, so that the original intermolecular hydrogen bonding of cellulose is broken, and the freed hydroxyl groups form stronger hydrogen bonds with the oxygen atoms in NMMO, and the fiber is fully dissolved; NMMO has strong water absorption and can form stable compounds with water. Therefore, when the water content increases, the sites available for hydrogen bonding on the NMMO molecules are occupied by water molecules, thereby reducing the dissolution ability of cellulose, and cellulose is gradually regenerated from the low concentration NMMO / water solution. The present invention selects dissolving pulp fibers, and innovatively uses a coating method to transfer the physical process of dissolution-regeneration of natural dissolving pulp cellulose fibers in different concentrations of NMMO / water solutions to the surface of the base paper, and at the same time, the regular physical structure of the regenerated cellulose and the rich surface hydroxyl groups are used to form a densely structured, fully biodegradable functional layer with barrier properties and reinforcement effects on the surface of the base paper.
[0011] Preferably, in the base paper layer of the fully biodegradable ultra-high barrier reinforced paper, the beating degree of conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood wood pulp, bamboo pulp, bagasse pulp, etc. is 30-55° SR.
[0012] Preferably, in the base paper layer of the fully biodegradable ultra-high barrier reinforced paper, the degree of substitution of the cationic modified microfibrillated cellulose is 5-9 mol% (the degree of substitution of the quaternary ammonium salt group is characterized by the content of amino groups), the diameter is 200-500 nm, and the aspect ratio is 50-300.
[0013] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, the mass ratio of the cationic modified microfibrillated cellulose to the conventional pulp fibers in the base paper layer is (1-6)%:(94-99)%.
[0014] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, in the coating liquid - NMMO / cellulose / water solution required for preparing the regenerated cellulose layer, the cellulose is selected from dissolving pulp fibers, and further, the dissolving pulp fibers can be selected from one of bleached coniferous wood dissolving pulp, bleached broadleaved wood dissolving pulp and bleached bamboo dissolving pulp; the mass concentration of cellulose in the coating liquid is 0.1-0.7%, and the mass concentration of NMMO is 70-90%.
[0015] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, the coating temperature during the coating process required for preparing the regenerated cellulose layer is 80-105°C.
[0016] Preferably, the preparation steps of the fully biodegradable ultra-high barrier reinforced paper include:
[0017] (1) crushing one or more conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood pulp, bamboo pulp, bagasse pulp, etc. into a pulp suspension with a mass concentration of 2 to 5%, and performing a pulping treatment to achieve a certain Schober beating degree;
[0018] (2) adding a certain mass percentage of cationic modified microfibrillated cellulose to the conventional pulp fiber suspension treated by pulping, diluting the mixed suspension to a mass concentration of 0.05-0.5%, and obtaining a base paper layer of a fully biodegradable ultra-high barrier reinforced paper after mechanical stirring, vacuum water filtration, forming, pressing and drum drying;
[0019] (3) preparing a certain mass concentration of NMMO / water solution, mixing a certain mass of dissolving pulp fibers with the NMMO / water solution, fully swelling under certain conditions and then stirring until completely dissolved, to obtain a NMMO / cellulose / water solution, wherein the swelling and dissolution conditions of the dissolving pulp fibers in the NMMO / water solution are a temperature of 80 to 105° C. and a time of 20 to 60 min;
[0020] (4) transferring the NMMO / cellulose / water solution to both sides of the base paper layer of the fully biodegradable ultra-high barrier reinforced paper by one of the coating methods selected from the group consisting of dipping, bar coating, curtain coating, or knife coating;
[0021] (5) The coated paper base material is immersed in distilled water at room temperature for 10 to 30 seconds to regenerate the dissolved cellulose pulp on the surface of the base paper layer, and then dried by a drum drying method or a flat plate drying method at a drying temperature of 85 to 105° C. for a drying time of 10 to 30 minutes to obtain a fully biodegradable ultra-high barrier reinforced paper.
[0022] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, the basis weight of the base paper layer is 40 to 200 g / m 2The coating amount of the regenerated cellulose layer is 0.05-1.00 g / m 2 .
[0023] The fully biodegradable ultra-high barrier reinforced paper provided by the present invention utilizes the physical properties of high aspect ratio and high specific surface area of the green, environmentally friendly and fully biodegradable cationic modified microfibrillated cellulose in the base paper layer to form a three-dimensional network structure that is intertwined and entangled with conventional pulp fibers, and the electrostatic binding force formed by chemical properties such as cations and conventional pulp fibers, thereby enhancing the mechanical strength performance of the base paper layer of the fully biodegradable ultra-high barrier reinforced paper. At the same time, a variety of coating methods are used to innovatively transfer the dissolution-regeneration process of regenerated cellulose fibers in NMMO / water solution to the surface of the paper base material (base paper layer), so as to form a layer of ultra-thin, dense physical structure, stable performance, ultra-high barrier performance (excellent water vapor barrier performance, oxygen barrier performance, low Cobb water absorption value and air permeability) and mechanical strength performance (high dry tensile strength, wet tensile strength and bursting strength) regenerated cellulose layer on the base paper layer. The NMMO solvent involved in the preparation method of the fully biodegradable ultra-high barrier reinforced paper provided by the present invention is green, environmentally friendly, safe, non-toxic, and easy to recycle, and the dissolution and recovery process is simple to operate, and does not involve dangerous operating conditions such as high temperature and high pressure. In addition, the fully biodegradable ultra-high barrier reinforced paper provided by the present invention only includes a base paper layer and a regenerated cellulose layer, and has a simple structure. Since the regenerated cellulose layer and the base paper layer are of the same origin, the fully biodegradable ultra-high barrier reinforced paper with a two-layer structure has excellent interlayer bonding performance due to the hydrogen bonding effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of the fully biodegradable ultra-high barrier reinforced paper prepared by the present invention
[0025] Figure 2 The preparation flow chart of the fully biodegradable ultra-high barrier reinforced paper of the present invention is DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings and the following embodiments to help those skilled in the art have a more complete, accurate and in-depth understanding of the inventive concept and technical solution of the present invention. It should be understood that the accompanying drawings and the following embodiments are only used to illustrate the present invention, rather than to limit the present invention.
[0027] In the description of the present invention, it should be noted that, if no specific conditions are specified in the examples, the experiments are carried out according to conventional conditions or conditions recommended by the manufacturer. The instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.
[0028] The conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood pulp, bamboo pulp, bagasse pulp, etc. of the present invention can be purchased from the market.
[0029] The cationic modified microfibrillar cellulose used in the present invention can be prepared by a quaternization reaction method, and the method used can be used as long as it can prepare the cationic modified microfibrillar cellulose. Reference can be made to published literature reports. For example, reference can be made to: Olszewska A, Eronen P, Johansson LS, et al. The behavior of cationic Nanofibrillar cellulose in aqueous media, 2011, 18 (5): 1213-1226; Master's thesis "Preparation of cationic modified microfibrillar cellulose and study on its ability to adsorb bile salts".
[0030] The dissolving pulp fiber and NMMO solvent of the present invention can be purchased from the market.
[0031] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0032] As attached Figure 1 As shown, the fully biodegradable ultra-high barrier reinforced paper of the present invention comprises a base paper layer 1, and a regenerated cellulose layer 2 and a regenerated cellulose layer 2 are respectively arranged on the upper surface and the lower surface of the base paper layer.
[0033] Specifically, in the present invention, the base paper layer 1 can be made by a rapid paper sheet forming method, and the regenerated cellulose layer 2 is prepared by a physical process of dissolution-regeneration of natural cellulose fibers in a NMMO / water solution.
[0034] Preferably, in the base paper layer 1 of the fully biodegradable ultra-high barrier reinforced paper, the beating degree of conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood wood pulp, bamboo pulp, bagasse pulp, etc. is 30-55° SR.
[0035] Preferably, in the base paper layer 1 of the fully biodegradable ultra-high barrier reinforced paper, the degree of substitution of the cationic modified microfibrillated cellulose is 5-9 mol% (the degree of substitution of the quaternary ammonium salt group is characterized by the content of amino groups), the diameter is 200-500 nm, and the aspect ratio is 50-300.
[0036] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, the mass ratio of the cationic modified microfibrillated cellulose to the conventional pulp fibers in the base paper layer 1 is (1-6)%:(94-99)%.
[0037] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, in the coating liquid - NMMO / cellulose / water solution required to prepare the regenerated cellulose layer 2, the cellulose is selected from dissolving pulp fibers, and further, the dissolving pulp fibers can be one of bleached coniferous wood dissolving pulp, bleached broadleaf wood dissolving pulp and bleached bamboo dissolving pulp; the mass concentration of cellulose in the coating liquid is 0.1-0.7%, and the mass concentration of NMMO is 70-90%.
[0038] Preferably, in the fully biodegradable ultra-high barrier reinforced paper, the coating temperature during the coating process required for preparing the regenerated cellulose layer 2 is 60-90°C.
[0039] Attached Figure 2 A preparation flow chart of the fully biodegradable ultra-high barrier reinforced paper of the present invention is provided.
[0040] Example 1
[0041] A fully biodegradable ultra-high barrier reinforced paper, the preparation method of which mainly comprises the following steps:
[0042] (1) 70 parts of bleached coniferous pulp and 30 parts of bleached hardwood pulp were mixed and crushed into a pulp suspension with a concentration of 3% by mass, and then subjected to low-consistency refining to a Schober beating degree of 30° SR;
[0043] (2) adding 8 mol% of cationic modified microfibrillated cellulose to the mixed pulp suspension having a Schober beating degree of 30°SR in an amount of 1.0% by mass of pulp fiber, and then diluting the mixed suspension to a mass concentration of 0.1%, and obtaining a base paper layer of a fully biodegradable ultra-high barrier reinforced paper after mechanical stirring, vacuum water filtration, forming, pressing and drum drying, and controlling the basis weight of the base paper to be 70 g / m 2 ;
[0044] (3) Preparation of NMMO / cellulose / water solution: 0.5‰ gallic acid was added to a 50% NMMO / water solution, and then concentrated to 78% by mass by rotary evaporation for 3 h; a certain amount of bleached softwood dissolving pulp fiber was weighed and added to the above 78% NMMO / water solution, stirred at 85°C for 30 min to fully swell, and then heated to 105°C and stirred for 10 min until completely dissolved to obtain a NMMO / cellulose / water solution, wherein the regenerated cellulose concentration was 0.5%;
[0045] (4) Use a scraper to coat once on a flat coater to transfer the NMMO / cellulose / water solution with a cellulose concentration of 0.5% to both sides of the base paper layer of the fully biodegradable ultra-high barrier reinforced paper. The temperature during the coating operation is 105°C, and the single-side coating amount is calculated to be 0.3 g / m 2 ;
[0046] (5) The coated paper base material is immersed in distilled water at room temperature for 10 seconds to allow the dissolved cellulose pulp to be regenerated on the surface of the base paper layer, and then the paper is drum dried at 85° C. for 10 minutes to obtain a fully biodegradable ultra-high barrier reinforced paper.
[0047] Example 2
[0048] A fully biodegradable ultra-high barrier reinforced paper:
[0049] The Schober beating degree of the pulp fiber raw material in step (1) is changed from 30°SR to 45°SR;
[0050] The degree of substitution of the cationic modified microfibrillated cellulose in step (2) was changed from 8 mol% to 6 mol%, and the addition amount was changed from 1.0% by weight of pulp fiber to 2.5% by weight;
[0051] The coating method of NMMO / cellulose / water solution in step (4) was changed from one coating on a flat coater using a scraper to one coating using a scraper, and the single-side coating amount was increased from 0.3 g / m 2 Change to 0.5g / m 2 ;
[0052] The remaining operations are the same as those in Example 1.
[0053] Example 3
[0054] A fully biodegradable ultra-high barrier reinforced paper:
[0055] The pulp fiber raw material in step (1) is changed from a mixture of 70 parts of bleached coniferous wood pulp and 30 parts of bleached broadleaf wood pulp to a mixture of 70 parts of bleached coniferous wood pulp and 30 parts of bleached bagasse pulp;
[0056] The degree of substitution of the cationic modified microfibrillated cellulose in step (2) was changed from 8 mol % to 5 mol %;
[0057] The remaining operations are the same as those in Example 1.
[0058] Example 4
[0059] A fully biodegradable ultra-high barrier reinforced paper:
[0060] The Schober beating degree of the pulp fiber raw material in step (1) is changed from 30°SR to 55°SR;
[0061] The basis weight of the base paper in step (2) was increased from 70 g / m 2 Change to 200g / m 2
[0062] The concentration of the NMMO / water solution in step (3) was changed from 78% to 85%, and the concentration of regenerated cellulose in the NMMO / cellulose / water solution was changed from 0.5% to 0.7%;
[0063] The coating method of NMMO / cellulose / aqueous solution in step (4) was changed from one-time coating on a flat coater using a scraper to dip coating, and the single-sided coating amount of NMMO / cellulose / aqueous solution was increased from 0.3 g / m 2 Changed to 1.0g / m 2 ;
[0064] The remaining operations are the same as those in Example 1.
[0065] Example 5
[0066] A fully biodegradable ultra-high barrier reinforced paper:
[0067] The basis weight of the base paper in step (2) was increased from 70 g / m 2 Change to 40g / m 2 ;
[0068] The single-sided coating amount of NMMO / cellulose / water solution in step (4) was increased from 0.3 g / m 2 Changed to 0.05g / m 2 ;
[0069] The remaining operations are the same as those in Example 1.
[0070] Example 6
[0071] A fully biodegradable ultra-high barrier reinforced paper:
[0072] The pulp fiber raw material in step (1) is changed from a mixture of 70 parts of bleached coniferous wood pulp and 30 parts of bleached broadleaf wood pulp to unbleached coniferous wood pulp;
[0073] The degree of substitution of the cationic modified microfibrillated cellulose in step (2) was changed from 8 mol% to 5 mol%, the addition amount was changed from 1.0% by weight of pulp fiber to 4% by weight, and the basis weight of the base paper was changed from 70 g / m 2 Changed to 120g / m 2 ;
[0074] The mass fraction of the concentrated NMMO / water solution in step (3) is changed from 78% to 90%, and the dissolving pulp fiber is changed from bleached coniferous wood dissolving pulp to bleached bamboo dissolving pulp;
[0075] The single-sided coating amount of NMMO / cellulose / water solution in step (4) was increased from 0.3 g / m 2 Changed to 0.1g / m 2 ;
[0076] The remaining operations are the same as those in Example 1.
[0077] Example 7
[0078] A fully biodegradable ultra-high barrier reinforced paper:
[0079] The pulp fiber raw material in step (1) is changed from a mixture of 70 parts of bleached coniferous wood pulp and 30 parts of bleached broadleaf wood pulp to unbleached coniferous wood pulp;
[0080] The degree of substitution of cationic modified microfibrillated cellulose in step (2) was changed from 8 mol% to 5 mol%, the addition amount was changed from 1.0% by weight of pulp fiber to 6% by weight, and the basis weight of base paper was changed from 70 g / m 2 Changed to 120g / m 2 ;
[0081] The dissolving pulp fiber in step (3) is changed from bleached coniferous wood dissolving pulp to bleached bamboo dissolving pulp;
[0082] The coating method of NMMO / cellulose / water solution in step (4) is changed from one-time coating on a flat coater using a doctor bar to curtain coating;
[0083] The remaining operations are the same as those in Example 1.
[0084] Example 8
[0085] A fully biodegradable ultra-high barrier reinforced paper:
[0086] The pulp fiber raw material in step (1) is changed from a mixture of 70 parts of bleached coniferous wood pulp and 30 parts of bleached broadleaf wood pulp to a mixture of 80 parts of bleached coniferous wood pulp and 20 parts of bleached bamboo pulp, and the Schober beating degree of the pulp fiber raw material is changed from 30°SR to 40°SR;
[0087] The degree of substitution of the cationic modified microfibrillated cellulose in step (2) was changed from 8 mol% to 9 mol%, the addition amount was changed from 1.0% by weight of pulp fiber to 3% by weight, and the basis weight of the base paper was changed from 70 g / m 2 Change to 100g / m 2 ;
[0088] The mass fraction of the concentrated NMMO / water solution in step (3) is changed from 78% to 87%, and the dissolving pulp fiber is changed from bleached coniferous wood dissolving pulp to bleached hardwood dissolving pulp;
[0089] The single-sided coating amount of NMMO / cellulose / water solution in step (4) was increased from 0.3 g / m 2 Change to 0.5g / m 2 ;
[0090] The remaining operations are the same as those in Example 1.
[0091] The fully biodegradable ultra-high barrier reinforced paper prepared according to the steps of Examples 1 to 8 was tested for relevant barrier properties and mechanical properties, and compared with the relevant technical indicators of standard QB / T 1014-2010 food packaging paper and the performance of three commercially available food packaging papers. The results are shown in the following table:
[0092]
[0093] It can be seen from the data in the table that by changing the key parameters such as pulp fiber type, beating degree, addition amount and substitution degree of cationic modified microfibrillated cellulose, and coating amount of different cellulose solutions, the ultra-high barrier reinforced paper obtained in Examples 1 to 8 is compared with the relevant technical indicators of food packaging paper in standard QB / T 1014-2010, and the performance of the ultra-high barrier reinforced paper prepared by the present invention far exceeds the standard requirements. In addition, compared with three commercially available food packaging papers, the ultra-high barrier reinforced paper prepared by the present invention has better performance in all aspects than the three commercially available food packaging papers.
[0094] The above preferred examples are only used to help explain the present invention, in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can better understand and use the present invention, and are not intended to limit the embodiments of the present invention. Obviously, various modifications and changes can be made according to the contents of this specification. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A fully biodegradable ultra-high barrier reinforced paper, characterized by: The fully biodegradable ultra-high barrier reinforced paper comprises a base paper layer and a regenerated cellulose layer, wherein the regenerated fiber layers are respectively arranged on the front and back sides of the base paper layer; wherein the base paper layer comprises one or more conventional pulp fibers such as unbleached or bleached coniferous wood pulp, broadleaf wood pulp, bamboo pulp, bagasse pulp, and cationic modified microfibrillated cellulose; and the regenerated fiber layer comprises regenerated cellulose fibers.
2. The fully biodegradable ultra-high barrier reinforced paper according to claim 1, characterized in that: In the base paper layer of the fully biodegradable ultra-high barrier reinforced paper, the beating degree of conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood wood pulp, bamboo pulp, bagasse pulp, etc. is 30-55° SR.
3. The fully biodegradable ultra-high barrier reinforced paper according to claim 1, characterized in that: In the base paper layer of the fully biodegradable ultra-high barrier reinforced paper, the degree of substitution of the cationic modified microfibrillated cellulose is 5-9 mol%, the diameter is 200-500 nm, and the aspect ratio is 50-300; the mass ratio of the cationic modified microfibrillated cellulose to conventional pulp fiber in the base paper layer is (1-6)%:(94-99)%.
4. The fully biodegradable ultra-high barrier reinforced paper according to claim 1, characterized in that: The basis weight of the base paper layer of the fully biodegradable ultra-high barrier reinforced paper is 40200 g / m 2 .
5. The fully biodegradable ultra-high barrier reinforced paper according to claim 1, characterized in that: In the regenerated cellulose layer of the fully biodegradable ultra-high barrier reinforced paper, in the coating liquid - NMMO / cellulose / water solution required for preparing the regenerated cellulose layer, the cellulose is selected from one of bleached coniferous wood dissolving pulp, bleached broadleaf wood dissolving pulp and bleached bamboo dissolving pulp; the mass concentration of cellulose in the coating liquid is 0.1-0.7%, and the mass concentration of NMMO is 70-90%.
6. The fully biodegradable ultra-high barrier reinforced paper according to claim 1, characterized in that: In the regenerated cellulose layer of the fully biodegradable ultra-high barrier reinforced paper, the coating temperature during the coating process required for preparing the regenerated cellulose layer is 80-105° C.; the coating amount of the regenerated cellulose layer is 0.05-1.00 g / m 2 .
7. A method for preparing fully biodegradable ultra-high barrier reinforced paper, characterized in that: The following steps are involved: (1) Pulp treatment: one or more conventional pulp fibers such as unbleached or bleached coniferous wood pulp, hardwood pulp, bamboo pulp, bagasse pulp, etc. are crushed into a pulp suspension with a mass concentration of 2 to 5%, and then subjected to pulping treatment; (2) Making the base paper layer: adding the cationic modified microfibrillated cellulose to the conventional pulp fiber suspension treated by pulping, diluting the mixed suspension to a mass concentration of 0.05-0.5%, and obtaining the base paper layer of the fully biodegradable ultra-high barrier reinforced paper after mechanical stirring, vacuum filtration, forming, pressing and drying; (3) Preparation of regenerated cellulose coating solution: preparing a certain mass concentration of NMMO / water solution, mixing a certain mass of dissolving pulp fibers with the NMMO / water solution, and stirring until completely dissolved after sufficient swelling to obtain a NMMO / cellulose / water solution; (4) coating treatment: transferring the NMMO / cellulose / water solution to both sides of the base paper layer of the fully biodegradable ultra-high barrier reinforced paper by one of the coating methods selected from the group consisting of dipping, bar coating, curtain coating, or knife coating; (5) Regeneration process of regenerated cellulose: The coated paper base material is immersed in distilled water at room temperature for 10 to 30 seconds to regenerate the dissolved cellulose pulp on the surface of the base paper layer, and then dried by drum drying or flat plate drying at a temperature of 85 to 105°C for a drying time of 10 to 30 minutes to obtain a fully biodegradable ultra-high barrier reinforced paper.
Citation Information
Patent Citations
Oil-proof food packaging paper and preparation method thereof
CN107574723A
Regenerated cellulose film coated green food packaging paper as well as preparation method and application thereof
CN112538777A
Preparation method of antibacterial fluoride-free oil-proof packaging paper
CN112796159A
Paper-made barrier packaging material and method for manufacturing the same
JP2013176949A