Method for observing and calculating activation energy of PET (Polyethylene Terephthalate) plastic
Through model-free combination method and microscopy technology, the change rate of the projection area of the ellipsoid was measured, combined with the Arenius formula, the difficulty of data monitoring and activation energy calculation during PET plastic hydrolysis was solved, and efficient and accurate activation energy observation was achieved. and calculate.
Patent Information
- Application Number
- CN202410840171.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-15
AI Technical Summary
The PET plastic hydrolysis process involves multiple chemical reactions, which makes it difficult to monitor data and calculate activation energy, and there are errors and inconveniences in existing methods.
The model-free method was used to measure the change rate of the ellipsoid projection area through drying pretreatment, thermogravimetric experimental analysis, and microscopy technology. The hydrolysis activation energy of PET plastic was calculated in combination with the Arenius formula, which reduced calculation errors and improved experiments. efficiency.
Microscopy technology accurately measures the size of the elliptical PET sample, quantitatively represents the hydrolysis rate through the change rate of the elliptical projection area, and calculates the activation energy using fitted linear images and Arenius formula, which improves the credibility and efficiency of the experiment.
Smart Images

Figure CN118961486A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PET plastics, in particular to a method for observing and calculating activation energy of PET plastics. Background Art
[0002] China is a major country in plastic production, consumption and recycling, with annual consumption ranking first in the world. Plastics have a short service life. In the context of mass plastic production, the green recycling of plastics has become a problem that needs to be solved, and it has also become an issue that needs attention. Polyethylene terephthalate (PET) has excellent physical, chemical and mechanical properties. It is widely used in the fields of fibers, bottles, films, etc. in the national economy. It is one of the most widely used and largest synthetic polymer materials; however, when the relative molecular weight of PET exceeds a certain value, it will show a higher viscosity and difficult processing and molding, which to a certain extent limits the further application of PET.
[0003] After searching, the Chinese patent number CN113188942A discloses a highly efficient calculation method for activation energy of thermal cracking of mixed plastics containing PVC, which has the application of the data processing part of the kinetic method analysis in the thermal cracking process of mixed plastics, and provides an analysis method for dividing the thermal cracking process of mixed plastics containing PVC into stages. The present invention selects an independent analysis method for the thermal cracking analysis curve of mixed plastics, and the calculation method of data processing adopts three model-free matching methods to calculate the activation energy in the thermal cracking of mixed plastics. The activation energy in the thermal cracking process of mixed plastics can be directly obtained without involving a kinetic model, thereby avoiding the error of the calculation result due to different assumed reaction mechanism functions, and reveals the relationship between the activation energy and conversion rate in the thermal cracking process of mixed plastics containing PVC, which is highly efficient and accurate.
[0004] However, the existing PET hydrolysis process involves multiple chemical reactions, and the overall process is difficult to monitor. Therefore, the relevant data and parameters are also difficult to capture, and various difficulties will arise in the subsequent calculation of the activation energy, which makes the observation and calculation of the activation energy also have certain inconveniences. Based on this, the present invention designs a method for observing and calculating the activation energy of PET plastics to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a method for observing and calculating the activation energy of PET plastic, which solves the experimental data problem in the background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for observing and calculating the activation energy of PET plastics, the specific steps are as follows:
[0008] S1, pretreatment and grouping, drying pretreatment of PET plastic, crushing and grinding, and weighing and grouping with a balance;
[0009] S2. Setting: setting the temperature rise range, temperature rise rate and experimental amount of each group of experimental samples for different groups of plastics;
[0010] S3, sealing, placing the prepared PET plastic in a glass tube with one end sealed by welding, injecting water, and sealing the other end by welding with hydrogen-oxygen flame;
[0011] S4, heating, placing the sealed glass tube on a hot and cold table for heating, performing a thermogravimetric analysis on the hydrolysis of the PET plastic, and obtaining a curve of the XPET of the PET at multiple heating rates versus the hydrolysis time and related experimental data;
[0012] S5. Observation: The hot and cold stages are placed under a microscope for real-time observation to obtain the rate of change of the PET ellipsoidal projection area, which is used to reflect the hydrolysis rate.
[0013] S6. Select data, select data corresponding to activation energy, use the formula to perform linear regression fitting, and obtain a fitted straight line image;
[0014] S7. Calculate the hydrolysis activation energy of PET by fitting the straight line graph and using the Arrhenius formula.
[0015] Preferably, in step S1, PET plastic is selected as a component of the experimental group, and the experimental samples are dried, crushed and ground for pretreatment, and then uniformly mixed according to a certain proportion and a certain amount of grams is selected and put into a crucible for the experiment, and the thermogravimetric analyzer is pre-set before the experiment.
[0016] Preferably, in step S2, under the saturated steam pressure, the temperature rising intervals are 25°C, 210°C, 240°C, 250°C, 260°C and 280°C respectively.
[0017] Preferably, in step S2, under the condition of saturated steam pressure and constant temperature of 320°C, the recorded hydrolysis times are 0 min, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min and 4 min, respectively.
[0018] Preferably, in step S3, the glass tube is made of quartz material, and the water content in the glass tube is approximately 2 / 3 of the volume of the glass tube.
[0019] Preferably, in step S2, the model of the hot and cold stage is Linkam CAP500, which can control the temperature reading of heating, and the heating rate is 20°C / min.
[0020] Preferably, the logic equation used in step S5 is used to analyze the decomposition process of the polymer, and its expression is as follows: The function x(t) is also called the S-type function, where x(t) represents the substance content at time t (i.e., the projected area of PET), k is the Malthusian parameter (maximum reaction rate), and the initial condition x(t=0) ranges from 0 to 1.
[0021] The three elements of thermal analysis kinetics research are activation energy, pre-exponential factor and mechanism function. The observation of activation energy is usually assumed to be a simple order reaction. The single heating rate method is used to obtain the apparent reaction order, activation energy and pre-exponential factor at a heating rate. The decomposition of activation energy is described by combining experimental data with model calculations, which is called the model matching method. In the process of model matching, it is inevitable that a variety of kinetic model functions will be generated, and these model functions can match the same reaction process curve. As one of the three elements of kinetics, activation energy is of great significance for accurately determining the pre-exponential factor and mechanism function of the thermal cracking process of PET plastics, as well as accurately explaining the reaction process. Therefore, this study is conducted.
[0022] PET hydrolysis is the process of dissolving a solid into a liquid. The kinetics of the PET hydrolysis reaction were evaluated in detail by measuring the volume change over time. Using microscopy, the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample were accurately measured, such as Figure 4 As shown. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the PET ellipsoidal projection area, and Table 1 lists the a-axis and b-axis lengths of PET at different temperatures and hydrolysis times.
[0023] Preferably, in step S7, the Arrhenius equation is, wherein k is the reaction rate, Q is the reaction activation energy (kJ·mol-1), R is the molar gas constant 8.314J·(mol·K)-1, T is the temperature (K), and A is the substance-specific pre-exponential coefficient.
[0024] Preferably, in step S4, as the hydrolysis reaction proceeds, the generated carboxyl terminal groups act as catalysts to accelerate the reaction. The carboxyl terminal groups promote the cleavage of ester bonds by providing protons, so as the carboxyl terminal groups accumulate, the reaction rate increases over time, thereby forming an autocatalytic cycle, and the autocatalytic effect causes the hydrolysis rate of PET to increase over time.
[0025] Preferably, in step S5, the microscopic technique can accurately measure the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the projected area of the PET ellipsoid.
[0026] The model-free matching method is also called the equal conversion rate method. The model-free matching method adopts the multi-heating rate method, that is, a method of performing thermal analysis kinetic processing under multiple heating rate curves.
[0027] The hydrolysis of PET has the characteristics of a typical autocatalytic process. In the hydrolysis mechanism of PET, autocatalysis plays a key role. As the reaction proceeds, the generated carboxyl terminal groups act as catalysts and accelerate the reaction. The carboxyl terminal groups promote the cleavage of ester bonds by providing protons. Therefore, as the carboxyl terminal accumulates, the reaction rate increases over time, forming an autocatalytic cycle. This autocatalytic effect causes the hydrolysis rate of PET to increase over time, rather than maintaining a constant rate.
[0028] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0029] 1. In the present invention, the microscopic technique can accurately measure the major and minor axis dimensions of the elliptical PET sample. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the projected area of the PET ellipsoid, which reduces the difficulty of observation and calculation and improves the experimental efficiency.
[0030] 2. The present invention uses the k value obtained by fitting the experimentally measured XPET and t data using a formula, and uses the Arrhenius formula to calculate the hydrolysis activation energy of PET. After fitting and calculation, the activation energy of ET hydrolysis is obtained. The use of the formula and the image improves the credibility of the experiment.
[0031] 2. The present invention obtains the rate of change of the ellipsoidal projection area of PET by real-time observation, thereby reflecting the hydrolysis rate. The data corresponding to the activation energy are selected, and a linear regression fitting is performed using a formula to obtain a fitted straight line image. The hydrolysis activation energy of PET is calculated using the Arrhenius formula through the fitted straight line image. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0033] Figure 2 It is a schematic diagram of the structure of the glass tube and the hot and cold stage;
[0034] Figure 3 It is a microscopic image of PET in the range of 25 to 280° C. under the steam saturation pressure of the present invention;
[0035] Figure 4 The microscopic images of PET at different hydrolysis times at 320° C. under the steam saturation pressure of the present invention;
[0036] Figure 5is the change of XPET of PET at different temperatures with hydrolysis time of the present invention;
[0037] Figure 6 is a fitted straight line graph of the Arrhenius formula of the present invention;
[0038] Figure 7 is the fitting reaction constant of PET hydrolysis at different temperatures. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Embodiment 1;
[0042] See also Figure 1-Figure 6 In an embodiment of the present invention, a method for observing and calculating the activation energy of PET plastics comprises the following specific steps:
[0043] S1, pretreatment and grouping, drying pretreatment of PET plastic, crushing and grinding, and weighing and grouping with a balance;
[0044] S2. Setting: setting the temperature rise range, temperature rise rate and experimental amount of each group of experimental samples for different groups of plastics;
[0045] S3, sealing, placing the prepared PET plastic in a glass tube with one end sealed by welding, injecting water, and sealing the other end by welding with hydrogen-oxygen flame;
[0046] S4, heating, placing the sealed glass tube on a hot and cold table for heating, performing a thermogravimetric analysis on the hydrolysis of the PET plastic, and obtaining a curve of the XPET of the PET at multiple heating rates as the hydrolysis time changes and related experimental data;
[0047] S5. Observation: The hot and cold stages are placed under a microscope for real-time observation to obtain the rate of change of the PET ellipsoidal projection area, which is used to reflect the hydrolysis rate.
[0048] S6. Select data, select data corresponding to activation energy, use the formula to perform linear regression fitting, and obtain a fitted straight line image;
[0049] S7. Calculate the hydrolysis activation energy of PET by fitting the straight line graph and using the Arrhenius formula.
[0050] like Figure 1As shown, in step S1, PET plastic is selected as the component of the experimental group. The experimental samples are dried, crushed and ground for pretreatment, and then mixed evenly according to the proportion. After that, a certain amount of grams is selected and put into the crucible for the experiment. The thermogravimetric analyzer is pre-set before the experiment.
[0051] like Figure 3 As shown, in step S2, under the saturated steam pressure, the temperature rising intervals are 25°C, 210°C, 240°C, 250°C, 260°C and 280°C respectively.
[0052] like Figure 4 As shown, in step S2, under the saturated steam pressure and a constant temperature of 320°C, the recorded hydrolysis times are 0 min, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min and 4 min, respectively.
[0053] like Figure 2 As shown, in step S3, the glass tube is made of quartz material, and the water content in the glass tube is approximately 2 / 3 of the volume of the glass tube.
[0054] The three elements of thermal analysis kinetics research are activation energy, pre-exponential factor and mechanism function. The observation of activation energy is usually assumed to be a simple order reaction. The single heating rate method is used to obtain the apparent reaction order, activation energy and pre-exponential factor at a heating rate. The decomposition of activation energy is described by combining experimental data with model calculations, which is called the model matching method. In the process of model matching, it is inevitable that a variety of kinetic model functions will be generated, and these model functions can match the same reaction process curve. As one of the three elements of kinetics, activation energy is of great significance for accurately determining the pre-exponential factor and mechanism function of the thermal cracking process of PET plastics, as well as accurately explaining the reaction process. Therefore, this study is conducted.
[0055] The working principle of the embodiment of the present invention is: first, pretreatment and grouping are carried out, PET plastic is dried and pretreated, and after crushing and grinding, it is weighed and grouped on a balance. PET plastic is selected as the component of the experimental group. After the experimental sample is dried, crushed and ground, it is uniformly mixed according to the proportion and the quantitative grams are selected and put into the crucible for the experiment. The thermogravimetric analyzer is pre-set before the experiment. Then the heating range, heating rate and experimental amount of each group of experimental samples of different groups of plastics are set. Under steam saturation pressure, the heating ranges are 25°C, 210°C, 240°C, 250°C, 260°C and 280°C respectively; under steam saturation pressure and constant temperature of 320°C, the recorded hydrolysis times are 0min, 0.5min, 1min, 1.5min, 2min, 2.5min, 3min and 4min respectively.
[0056] The prepared PET plastic is placed in a glass tube with one end sealed by welding, and water is poured in. The other end is sealed by welding with an oxyhydrogen flame. The sealed glass tube is placed on a hot and cold table for heating, and the hydrolysis of the PET plastic is analyzed by thermogravimetric experiments. The change curves of XPET of PET at multiple heating rates with hydrolysis time and related experimental data are obtained.
[0057] Embodiment 2;
[0058] See also Figure 1-Figure 6 In the embodiment of the present invention, in step S2, the model of the hot and cold stage is LinkamCAP500, which can control the temperature reading of heating, and the heating rate is 20°C / min.
[0059] The logic equation used in step S5 is used to analyze the decomposition process of the polymer, and its expression is as follows: The function x(t) is also called the S-type function, where x(t) represents the substance content at time t (i.e., the projected area of PET), k is the Malthusian parameter (maximum reaction rate), and the initial condition x(t=0) ranges from 0 to 1.
[0060] The model-free matching method is also called the equal conversion rate method. The model-free matching method adopts the multi-heating rate method, that is, a method of performing thermal analysis kinetic processing under multiple heating rate curves.
[0061] The working principle of the embodiment of the present invention is: the hot and cold stage is placed under a microscope, and real-time observation is performed to obtain the rate of change of the PET ellipsoidal projection area, thereby reflecting the hydrolysis rate. Data corresponding to the activation energy are selected, and a linear regression fitting is performed using a formula to obtain a fitted straight line image. By fitting the straight line image, the hydrolysis activation energy of PET is calculated using the Arrhenius formula.
[0062] PET hydrolysis is the process of dissolving a solid into a liquid. The kinetics of the PET hydrolysis reaction were evaluated in detail by measuring the volume change over time. Using microscopy, the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample were accurately measured, such as Figure 4 As shown. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the PET ellipsoidal projection area, and Table 1 lists the a-axis and b-axis lengths of PET at different temperatures and hydrolysis times.
[0063] Embodiment 3;
[0064] See also Figure 1-Figure 6 In the embodiment of the present invention, in step S7, the Arrhenius formula is
[0065] Where k is the reaction rate and Q is the reaction activation energy (kJ·mol -1), R is the molar gas constant 8.314 J·(mol·K)- 1 , T is temperature (K), and A is the substance-specific pre-exponential coefficient.
[0066] In step S4, as the hydrolysis reaction proceeds, the generated carboxyl terminal groups act as catalysts to accelerate the reaction. The carboxyl terminal groups promote the cleavage of ester bonds by providing protons, so as the carboxyl terminal groups accumulate, the reaction rate increases over time, thereby forming an autocatalytic cycle, and the autocatalytic effect causes the hydrolysis rate of PET to increase over time.
[0067] In step S5, the microscopy technique can accurately measure the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the projected area of the PET ellipsoid.
[0068] The working principle of the embodiment of the present invention is: Figure 5 The relationship between the projected area of PET and time is shown. The dissolution kinetics of PET show a trend of slow first, fast, and then slow again. This pattern is very consistent with the logistic model. The logistic equation has been used to analyze the decomposition process of polymers, which is expressed as follows:
[0069]
[0070] The function x(t) is sometimes called an S-type function, where x(t) represents the substance content at time t (i.e., the projected area of PET), k is the Malthusian parameter (maximum reaction rate), and the initial condition x(t=0) ranges from 0 to 1. The data points in Table 1 are fitted according to the formula.
[0071] The hydrolysis of PET has the characteristics of a typical autocatalytic process. In the hydrolysis mechanism of PET, autocatalysis plays a key role. As the reaction proceeds, the generated carboxyl terminal groups act as catalysts and accelerate the reaction. The carboxyl terminal groups promote the cleavage of ester bonds by providing protons. Therefore, as the carboxyl terminal accumulates, the reaction rate increases over time, forming an autocatalytic cycle. This autocatalytic effect causes the hydrolysis rate of PET to increase over time, rather than maintaining a constant rate.
[0072] Working principle: First, pretreatment and grouping are carried out. PET plastic is dried and pretreated. After crushing and grinding, it is weighed and grouped on a balance. PET plastic is selected as the component of the experimental group. After drying, crushing and grinding the experimental samples, they are evenly mixed according to the proportion and the quantitative grams are selected and put into the crucible for the experiment. The thermogravimetric analyzer is pre-set before the experiment. Then the heating range, heating rate and experimental amount of each group of experimental samples of different groups of plastics are set. Under steam saturation pressure, the heating ranges are 25℃, 210℃, 240℃, 250℃, 260℃ and 280℃ respectively; under steam saturation pressure and constant temperature of 320℃, the recorded hydrolysis times are 0min, 0.5min, 1min, 1.5min, 2min, 2.5min, 3min and 4min respectively.
[0073] The prepared PET plastic is placed in a glass tube with one end sealed by welding, and water is poured in. The other end is sealed by welding with an oxyhydrogen flame. The sealed glass tube is placed on a hot and cold table for heating, and the hydrolysis of the PET plastic is analyzed by thermogravimetric experiments. The change curves of XPET of PET at multiple heating rates with hydrolysis time and related experimental data are obtained.
[0074] The hot and cold stages are placed under a microscope for real-time observation to obtain the rate of change of the PET ellipsoidal projection area, which reflects the hydrolysis rate. The data corresponding to the activation energy are selected and linear regression fitting is performed using the formula to obtain a fitted straight line image. The hydrolysis activation energy of PET is calculated using the Arrhenius formula by fitting the straight line image.
[0075] PET hydrolysis is the process of dissolving a solid into a liquid. The kinetics of the PET hydrolysis reaction were evaluated in detail by measuring the volume change over time. Using microscopy, the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample were accurately measured, such as Figure 4 As shown. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the PET ellipsoidal projection area, and Table 1 lists the a-axis and b-axis lengths of PET at different temperatures and hydrolysis times.
[0076] Figure 5 The relationship between the projected area of PET and time is shown. The dissolution kinetics of PET show a trend of slow first, fast, and then slow again. This pattern is very consistent with the logistic model. The logistic equation has been used to analyze the decomposition process of polymers, which is expressed as follows:
[0077]
[0078] The function x(t) is sometimes called an S-type function, where x(t) represents the substance content at time t (i.e., the projected area of PET), k is the Malthusian parameter (maximum reaction rate), and the initial condition x(t=0) ranges from 0 to 1. The data points in Table 1 are fitted according to the formula.
[0079] The hydrolysis of PET has the characteristics of a typical autocatalytic process. In the hydrolysis mechanism of PET, autocatalysis plays a key role. As the reaction proceeds, the generated carboxyl terminal groups act as catalysts and accelerate the reaction. The carboxyl terminal groups promote the cleavage of ester bonds by providing protons. Therefore, as the carboxyl terminal accumulates, the reaction rate increases over time, forming an autocatalytic cycle. This autocatalytic effect causes the hydrolysis rate of PET to increase over time, rather than maintaining a constant rate.
[0080] The experimentally measured XPET and t data ( Figure 5 ) and the k values obtained by fitting the formula are shown in Table 1. The hydrolysis activation energy (Q) of PET can be calculated using the Arrhenius formula.
[0081]
[0082] Where k is the reaction rate and Q is the reaction activation energy (kJ·mol -1 ), R is the molar gas constant 8.314 J·(mol·K) -1 , T is temperature (K), and A is the substance-specific pre-exponential coefficient.
[0083] pass Figure 6 The obtained lnk-1 / T plot was analyzed to determine the activation energy (Q) of PET hydrolysis, and the Q value was found to be 134.89 kJ·mol-1 in the temperature range of 280-330 °C.
[0084] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and alterations may be made to the embodiments without departing from the principles and spirit thereof, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for observing and calculating the activation energy of PET plastics, characterized in that The specific steps are as follows: S1, pretreatment and grouping, drying pretreatment of PET plastic, crushing and grinding, and weighing and grouping with a balance; S2. Setting: setting the temperature rise range, temperature rise rate and experimental amount of each group of experimental samples for different groups of plastics; S3, sealing, placing the prepared PET plastic in a glass tube sealed at one end, injecting water, and sealing the other end with a hydrogen-oxygen flame; S4, heating, placing the sealed glass tube on a hot and cold table for heating, performing a thermogravimetric analysis on the hydrolysis of the PET plastic, and obtaining a curve of the XPET of the PET at multiple heating rates versus the hydrolysis time and related experimental data; S5. Observation: The hot and cold stages are placed under a microscope for real-time observation to obtain the rate of change of the PET ellipsoidal projection area, which is used to reflect the hydrolysis rate. S6. Select data, select data corresponding to activation energy, use the formula to perform linear regression fitting, and obtain a fitted straight line image; S7. Calculate the hydrolysis activation energy of PET by fitting the straight line graph and using the Arrhenius formula.
2. The method for observing and calculating the activation energy of PET plastic according to claim 1, characterized in that: In step S1, PET plastic is selected as the component of the experimental group. The experimental samples are dried, crushed and ground for pretreatment, and then uniformly mixed according to the proportion and a certain amount of grams are selected and put into the crucible for the experiment. The thermogravimetric analyzer is pre-set before the experiment.
3. The method for observing and calculating the activation energy of PET plastic according to claim 1, characterized in that: In step S2, under the saturated steam pressure, the temperature rising intervals are 25°C, 210°C, 240°C, 250°C, 260°C and 280°C respectively.
4. The method for observing and calculating the activation energy of PET plastic according to claim 1, characterized in that: In step S2, under the saturated steam pressure and constant temperature of 320°C, the recorded hydrolysis times were 0 min, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min and 4 min, respectively.
5. The method for observing and calculating the activation energy of PET plastic according to claim 1, characterized in that: In step S3, the glass tube is made of quartz material, and the water content in the glass tube is about 2 / 3 of the volume of the glass tube.
6. The method for observing and calculating activation energy of PET plastic according to claim 1, characterized in that: In step S2, the model of the hot and cold stage is Linkam CAP500, which can control the temperature reading of heating, and the heating rate is 20°C / min.
7. The method for observing and calculating activation energy of PET plastic according to claim 1, characterized in that: The logic equation used in step S5 is used to analyze the decomposition process of the polymer, and its expression is as follows: The function x(t) is also called the S-type function, where x(t) represents the substance content at time t (i.e., the projected area of PET), k is the Malthusian parameter (maximum reaction rate), and the initial condition x(t=0) ranges from 0 to 1.
8. The method for observing and calculating activation energy of PET plastic according to claim 1, characterized in that: In step S7, the Arrhenius formula is Where k is the reaction rate and Q is the reaction activation energy (kJ·mol -1 ), R is the molar gas constant 8.314 J·(mol·K) -1 , T is temperature (K), and A is the substance-specific pre-exponential coefficient.
9. The method for observing and calculating activation energy of PET plastic according to claim 1, characterized in that: In step S4, as the hydrolysis reaction proceeds, the generated carboxyl terminal groups act as catalysts to accelerate the reaction. The carboxyl terminal groups promote the breaking of ester bonds by providing protons. Therefore, as the carboxyl terminal groups accumulate, the reaction rate increases over time, thereby forming an autocatalytic cycle. The autocatalytic effect causes the hydrolysis rate of PET to increase over time.
10. The method for observing and calculating activation energy of PET plastic according to claim 1, characterized in that: In step S5, the microscopy technique can accurately measure the major axis (a-axis) and minor axis (b-axis) dimensions of the elliptical PET sample. Since a uniform hydrolysis rate is observed in each direction of the PET solid, the hydrolysis rate can be quantitatively expressed by the rate of change of the projected area of the PET ellipsoid.