Grating impressing method based on thickness adjustment and diffraction optical waveguide

Through thickness adjustment and surface treatment technology, the problem of uneven optical performance in different areas of the substrate in nanoimprinting technology is solved, and the optical performance and the printing quality are improved, ensuring high-quality transfer of products.

CN118963060APending Publication Date: 2024-11-15SHANGHAI NORTH OCEAN TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411376989.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-15

Smart Images

  • Figure CN118963060A_ABST
    Figure CN118963060A_ABST
Patent Text Reader

Abstract

The invention provides a grating impressing method based on thickness adjustment and a diffraction optical waveguide, and the method comprises the steps: detecting the spin coating thickness values of an impressing glue layer at different region positions after the spin coating of a substrate, respectively judging the target spin coating thickness of the impressing glue layer before impressing, and calculating the determined target spin coating thickness; the processed imprinting glue layer is imprinted through a working template with a smooth surface, so that the distance between the working template and the substrate is controlled to be the target glue uniformizing thickness, the smooth surface has a preset surface contact angle, the working template is conveniently removed, and finally the imprinting technology is carried out through the imprinting mother set. The thickness of the impressing residual adhesive layer of the obtained product at different positions of the substrate has good consistency, and the optical performance of the product in the middle of the substrate can be improved; therefore, the optical performance of the diffraction optical waveguide formed by imprinting on the whole substrate is improved, the quality of the whole imprinting process is improved in this way, the transfer of the optical micro-nano structure is realized, and the qualified rate of products is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nanoimprint technology, and in particular to a grating imprint method based on thickness adjustment and a diffraction optical waveguide. Background Art

[0002] Diffractive optical waveguides are one of the important optical devices in the field of augmented reality display technology. In the prior art, diffractive optical waveguides are often mass-produced by nanoimprinting technology. In order to improve the efficiency of mass production, multi-mesh diffractive optical waveguides are often imprinted on the surface of a wafer substrate, such as diffractive optical waveguides with four, six, eight, etc. meshes, so as to form a multi-mesh diffractive optical waveguide product through a single imprinting process.

[0003] However, when testing the optical performance of multiple diffraction optical waveguide products formed on the surface of the same wafer substrate, technicians in this field found that the optical performance of the diffraction optical waveguide formed in the middle of the same wafer substrate is generally lower than that of the diffraction optical waveguide in other areas, such as optical efficiency, uniformity and other optical performance parameters. It was even further found that in some different imprinting processes, the optical performance of the diffraction optical waveguide in the middle area of ​​the same wafer substrate and other areas is quite different. This will greatly reduce the yield of the product, which is undesirable for technicians in this field.

[0004] How to improve the existing embossing process to improve the optical performance of products in different areas is an urgent problem to be solved. Summary of the invention

[0005] The present invention provides a grating imprinting method and a diffractive optical waveguide based on thickness adjustment, in the hope of improving the existing imprinting process, so as to improve the optical performance of the diffractive optical waveguide in different areas of the same substrate, especially to improve the imprinting quality of the middle area of ​​the substrate.

[0006] A grating imprinting method based on thickness adjustment comprises the following steps:

[0007] (1) providing a substrate, coating a predetermined thickness of embossing adhesive on the surface of the substrate, and evenly coating the embossing adhesive to form an embossing adhesive layer;

[0008] (2) detecting the thickness of the embossed adhesive layer after coating, and determining the thickness of the embossed adhesive layer in different areas;

[0009] (3) determining a target coating thickness of the embossed adhesive layer according to the thickness of the embossed adhesive layer in different regions determined in step (2);

[0010] (4) providing a working template, and performing surface treatment on any smooth surface of the working template so that the surface contact angle of the surface is greater than a preset value, thereby obtaining a smooth surface;

[0011] (5) using the working template in step (4) to emboss the embossed adhesive layer, with the smooth surface of the working template facing the embossed adhesive layer; and performing embossing so that the distance between the working template and the substrate is equal to the target adhesive thickness in step (3);

[0012] (6) removing the working template, and detecting the thickness of the embossed adhesive layer after embossing based on the same method as step (2), and judging whether the adhesive thickness of different regions meets the target adhesive thickness; if so, proceeding to the next step; otherwise, repeating step (5) until the thickness of the embossed adhesive layer after embossing meets the target adhesive thickness;

[0013] (7) Based on a preset imprinting master, imprinting the imprinting glue layer in step (6), wherein the imprinting master has a graphic structure to be transferred by imprinting; after curing, removing the imprinting master to obtain a grating imprinting structure.

[0014] In the step (1), before coating the embossing adhesive, the surface of the substrate is subjected to plasma treatment, and a layer of adhesion promoter is disposed on the surface after the plasma treatment.

[0015] Furthermore, in step (1), the substrate is a transparent substrate, which may be a glass wafer, a resin wafer, a silicon carbide wafer, etc. The predetermined thickness of the embossed adhesive layer is limited to 30 nm to 300 nm.

[0016] In step (1), a spin coating process is adopted with a rotation speed of 1000 rpm to 3000 rpm to achieve a uniform coating operation.

[0017] Furthermore, in step (2), the thickness of the printed adhesive layer after the coating is performed is detected by optical means, such as an ellipsometer, a laser rangefinder or other optical device capable of detecting nanometer-level distances.

[0018] Furthermore, in the step (2), at least the thickness of N regions of the embossed adhesive layer is detected, where N is ≥ 3 and is a natural number.

[0019] In step (3), the target thickness of the embossed adhesive layer is determined based on the thickness of the embossed adhesive layer in different regions determined in step (2), and the minimum value of the target thickness meets the height requirement of the embossed micro-nano structure.

[0020] Furthermore, in the step (3), based on the thickness H of the embossed adhesive layer in different regions N , determine the minimum value of the thickness of the plurality of embossed adhesive layers, and determine the target adhesive thickness H of the embossed adhesive layer based on the minimum value of the thickness of the embossed adhesive layer measured in different regions, H≥min(H 1 , H 2 ,......H N ).

[0021] In some other embodiments, the thickness H of the embossed adhesive layer in different regions is N , the target uniform coating thickness H of the embossed adhesive layer is not greater than the average thickness of the embossed adhesive layer in different regions, H≤(H 1 +H 2 ......+H N ) / N.

[0022] In the above embodiment, H 1 , H 2 ,......H N They respectively represent the thickness of the imprinted glue layer in different areas; and the minimum value of the target glue thickness H meets the height requirement of the imprinted grating structure.

[0023] Furthermore, in the step (4), the surface contact angle is not less than 105°, so that the smooth surface has good hydrophobicity.

[0024] Practically, the target coating thickness H is limited to a range of 30 nm to 300 nm.

[0025] Optionally, in step (5), force is uniformly applied to the working template so that the smooth surface of the working template acts uniformly on various areas of the embossed adhesive layer, so that the distance between the working template and the substrate is controlled to be the target adhesive thickness determined in the previous step.

[0026] Furthermore, in some other embodiments, in step (6), when the thickness of each different area does not meet the preset target glue thickness, step (5) is repeated, and it also includes selecting different areas to re-coat the embossed glue based on the thickness of different areas to perform the operation of step (5) again.

[0027] The present invention provides a diffractive optical waveguide, which is prepared by a grating imprinting method based on thickness adjustment according to any of the aforementioned embodiments.

[0028] In the present invention, through the aforementioned steps, firstly, the thickness of the embossed glue layer in different glue-leveling areas is judged, and the target glue-leveling thickness of the glue layer to be embossed is judged and calculated according to the thickness of the embossed glue layer in different glue-leveling areas, which can be calculated according to different methods; of course, the minimum value of the target glue-leveling thickness H meets the height requirement of the embossed grating structure; and the target glue-leveling thickness is realized and controlled by the surface-treated working template, thereby realizing the adjustment of the glue-leveling thickness, thereby realizing the uniformity control of the thickness of the embossed glue layer, so that the thickness of the embossed glue layer in each area is kept as the same as possible; the method of the present invention can improve the problem of uneven glue-leveling thickness at high rotation speed, thereby improving the subsequent imprinting process and improving the imprinting quality.

[0029] After improving the uniformity of the glue thickness, embossing is performed. After testing, the diffractive optical waveguide product obtained after embossing can significantly improve the uniformity of the thickness of the embossed residual glue, so that the thickness of the embossed residual glue layer in the middle area and other areas of the substrate surface is as consistent as possible, and the optical performance of the formed diffractive optical waveguide is improved, especially for the diffractive optical waveguide product formed in the middle part of the substrate, so that the optical performance of the diffractive optical waveguide is closer to that of the diffractive optical waveguide in other areas, and the performance of the diffractive optical waveguide formed by embossing on the entire substrate is improved, and a good efficiency uniformity is maintained. In this way, the quality of the entire embossing process is improved, and high-quality embossing transfer of micro-nano structures is achieved, thereby improving the product qualification rate and display efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 It is a schematic diagram of a multi-eye diffraction optical waveguide structure arranged on a substrate in the prior art shown in the present invention;

[0032] Figure 2 It is a schematic diagram of uneven thickness on a substrate after coating according to the present invention;

[0033] Figure 3 A schematic diagram of the thickness of an embossed adhesive layer after embossing a working template provided by the present invention;

[0034] Figure 4 A schematic diagram of a working template structure provided by the present invention;

[0035] Figure 5 A schematic diagram of a structure of a rubber layer embossed by a working template provided by the present invention;

[0036] Figure 6 A schematic diagram of the structure of performing imprinting by an imprinting master provided by the present invention;

[0037] Figure 7 A schematic flow chart of a grating imprinting method based on thickness adjustment provided by the present invention. DETAILED DESCRIPTION

[0038] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0039] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0040] like Figure 1 As shown in the figure, multiple diffractive optical waveguide products are often formed by embossing on the same wafer substrate surface; due to the embossing process, the optical performance of the diffractive optical waveguide formed in the middle area of ​​the substrate surface is generally lower than that of the diffractive optical waveguide in other areas, such as Figure 1 The area shown in the dotted box in the middle shows that the optical performance of the waveguide formed in this area is significantly lower than that in other areas after testing after imprinting and cutting. After SEM testing of the sample, the uneven thickness of the imprinted adhesive layer remaining after imprinting may be one of the reasons for the inconsistent optical performance.

[0041] In order to improve the optical performance of the embossed product in the middle area of ​​the substrate surface, the present invention provides the following method.

[0042] A grating imprinting method based on thickness adjustment comprises the following steps:

[0043] (1) providing a substrate, coating a predetermined thickness of embossing adhesive on the surface of the substrate, and evenly coating the embossing adhesive to form an embossing adhesive layer;

[0044] (2) Detecting the thickness of the embossed adhesive layer after coating, and determining the thickness of the embossed adhesive layer in different areas;

[0045] (3) determining a target coating thickness of the embossed adhesive layer according to the thickness of the embossed adhesive layer in different regions determined in step (2);

[0046] (4) providing a working template, and performing surface treatment on any smooth surface of the working template so that the surface contact angle of the surface is greater than a preset value, thereby obtaining a smooth surface;

[0047] (5) using the working template in step (4) to emboss the embossed adhesive layer, with the smooth surface of the working template facing the embossed adhesive layer; and performing embossing so that the distance between the working template and the substrate is equal to the target adhesive thickness in step (3);

[0048] (6) removing the working template, and detecting the thickness of the embossed adhesive layer after embossing based on the same method as step (2), and judging whether the adhesive thickness of different regions meets the target adhesive thickness; if so, proceeding to the next step; otherwise, repeating step (5) until the thickness of the embossed adhesive layer after embossing meets the target adhesive thickness;

[0049] (7) Based on a preset imprinting master, imprinting the imprinting glue layer in step (6), wherein the imprinting master has a graphic structure to be transferred by imprinting; after curing, removing the imprinting master to obtain a grating imprinting structure.

[0050] In detail, the present invention will be further described below.

[0051] Further, in step (1), if Figures 2-3 As shown, the substrate 10 is a transparent substrate, which may be a glass wafer, a resin wafer, a silicon carbide wafer, etc. The predetermined thickness of the embossed adhesive layer is limited to 30 nm to 300 nm.

[0052] In step (1), a predetermined thickness of an embossed adhesive layer 20 is coated on the surface of a substrate 10 by spin coating at a rotation speed of 1000 rpm to 3000 rpm to achieve a uniform coating operation.

[0053] Furthermore, in step (2), the thickness of the printed adhesive layer after the coating is performed is detected by optical means, such as an ellipsometer, a laser rangefinder or other optical device capable of detecting nanometer-level distances.

[0054] like Figure 2As shown in FIG. , based on the glue-spinning operation of step (1), usually, since the environment medium of glue-spinning is air environment, the air flow at different positions of the substrate is likely to cause different or slightly changing air pressures at different positions of the substrate under high-speed rotation. These changing airflows are likely to cause the thickness of the embossed glue on the surface of the substrate to change, forming an uneven glue layer surface, such as Figure 2 A plurality of embossed adhesive layers with different heights are formed, such as a layer with a thickness of H 1 , H 2 , H 3 , H 4 , H 5 ; Figure 2 The figure shows the changes of the embossed adhesive on the substrate surface after coating under different air pressure conditions, such as the thickness decreasing from the middle of the substrate to the edge of the substrate, H 1 >H 2 , H 1 >H 3 , H 1 >H 4 , H 1 >H 5 Of course, in other cases, such as H 1 <H 2 , H 1 <H 3 , H 1 <H 4 , H 1 <H 5 ; etc. Figure 2 Only two cases of changes after coating are shown. Of course, there are other cases of changes in coating thickness under different air pressure conditions. The present invention does not list them one by one, and they are all in the embodiments defined in the present invention. Figure 2 It does not constitute a limitation on the thickness change of the printed adhesive layer after coating. Different coating environments will lead to different thickness changes.

[0055] Further, in step (2), the thickness of the embossed adhesive layer in different areas of the substrate surface after the adhesive is applied is detected, and it is limited to detect the thickness of at least N areas, where N ≥ 3 and is a natural number, that is, H 1 , H 2 ,......H N ; They represent the thickness of the embossed adhesive layer in different regions, such as the thickness of the first region H 1 , the thickness of the second region H 2 ...the thickness of the Nth region is H N ; As an example, it is defined as N=5, including H 1 , H 2 , H 3 , H 4 , H 5Of course, the number of test areas on the substrate surface can be selected according to actual conditions, such as 6, 8, 12, etc., to achieve accurate measurement.

[0056] Further, in step (3), the target thickness of the embossed adhesive layer is determined according to the thickness of the embossed adhesive layer in different regions determined in step (2). In more detail, two methods are included. For example, method 1 determines the minimum value of the thickness of multiple embossed adhesive layers based on the thickness of the embossed adhesive layer in different regions, such as H≥min(H 1 , H 2 ,......H N ), based on the minimum value of the measured thickness of the embossed adhesive layer in different areas, the target thickness of the embossed adhesive layer is determined, that is, the target thickness of the embossed adhesive layer is H≥min(H 1 , H 2 ,......H N ), in this method, the minimum thickness of the imprinted adhesive layer detected is used as the parameter of the target adhesive thickness to achieve uniform thickness in each area, which is conducive to ensuring the continuity and integrity of the imprinted structure in the subsequent imprinting steps. Of course, the specific size of H can be limited based on the imprinted micro-nano structure. At the same time, the minimum value of the target adhesive thickness needs to be greater than the height of the grating structure formed by the imprinting and the thickness of the imprinted residual adhesive layer, which can be determined.

[0057] It can be known that in step (3), the target thickness of the embossed adhesive layer is determined according to the thickness of the embossed adhesive layer in different areas determined in step (2), and the minimum value of the target thickness needs to meet the height requirement of the embossed micro-nano structure; if the minimum value of the target thickness meets the height requirement of the embossed grating structure, further, if the minimum value of the target thickness needs to be greater than the height of the grating structure formed by the embossing and the thickness of the residual adhesive layer formed by the embossing.

[0058] It can be seen that the range of the target coating thickness H is limited to 30 nm to 300 nm.

[0059] In another method, method 2, based on the thickness H of the embossed adhesive layer in different regions 1 , H 2 ,......H N , the target thickness of the embossed adhesive layer is limited to not more than the average thickness of the embossed adhesive layer in different regions, such as H≤(H 1 +H 2 ......+H N) / N, based on the subsequent steps, the embossed adhesive layer is embossed by the working template, which facilitates the flow between different areas of the embossed adhesive layer, which is conducive to the thickness control of the embossed adhesive layer between different areas, especially for areas with smaller thickness of the embossed adhesive layer, the thickness of the embossed adhesive layer in different areas is uniformized by the flow of the embossed adhesive in other areas, which can ensure the uniformity of thickness between different areas and improve the quality of embossing. Of course, the specific size of H can be limited based on the embossed micro-nano structure. At the same time, the minimum value of the target uniform adhesive thickness needs to be greater than the height of the grating structure formed by the embossing and the thickness of the embossed residual adhesive layer, which can be determined.

[0060] In the above embodiment, H 1 , H 2 ,......H N They respectively represent the thickness of the embossed rubber layer in different areas.

[0061] In step (3), two different methods for controlling the thickness of the embossed adhesive layer to be uniform can be used to accurately control the thickness between different regions, so that the uniformity and stability of the embossed adhesive residue can be ensured as much as possible after the grating structure is formed by embossing.

[0062] Furthermore, in step (4), if Figure 4 As shown, a working template 30 is provided, such as PET, aluminum plate, steel plate, hard glass, etc., whose elastic modulus is not less than 30Gpa; the working template 30 has at least one smooth surface, and the smooth surface is surface treated so that the surface contact angle of the surface is greater than a preset value to obtain a smooth surface 310; such as chemical surface treatment, physical surface treatment, etc. in the art, the present invention does not make any limitation to this, that is, as long as the surface contact angle of the smooth surface 310 can be made greater than the preset value, such as the surface contact angle is not less than 105°, such as 110°~130°, 130°~150° or 150°~160°, etc. By controlling the contact angle of the working template surface, the smooth surface 310 of the working template 30 has good hydrophobicity, and liquid or impurities are not easy to deposit on the surface. In the subsequent process steps, it is easier to remove the working template, prevent the embossed glue from sticking to the surface of the working template, etc., so as to facilitate the separation of the surface of the working template and the embossed glue layer, reduce the force between the two, and then ensure the surface thickness of the embossed glue layer and the integrity of the glue layer plane.

[0063] In the present invention, the working template is used to emboss the embossed adhesive layer 20 so as to adjust the thickness of different regions of the embossed adhesive layer 20 to be uniform.

[0064] In some embodiments, further, step (5) is included, in which the working template in step (4) is used to imprint the imprinted adhesive layer 20 in step (3). During the process, the smooth surface 310 of the working template 30 is limited to face the imprinted adhesive layer 20; and the imprinting is performed so that the distance between the working template 30 and the substrate 10 is the target adhesive thickness H in step (3).

[0065] In this step, the force F is evenly applied to each area of ​​the working template 30, so that the smooth surface 310 of the working template 30 evenly acts on each area of ​​the embossed adhesive layer 20, so that the distance between the working template 30 and the substrate 10 is controlled to be the target adhesive thickness H determined in the previous step. The adhesive thickness of the embossed adhesive layer can be controlled by moving the distance of the working template 30, which can improve the problem of uneven adhesive thickness at high speed, thereby improving the subsequent embossing process and improving the embossing quality. In this process step, the force F needs to be evenly applied to each area of ​​the working template 30 to prevent the embossed adhesive layer from flowing randomly, thereby affecting the thickness of different areas.

[0066] In step (5), after the working template 30 has been evenly applied to each area of ​​the embossed adhesive layer 20 for a certain period of time, the next step is performed.

[0067] Step (6), remove the working template 30, and detect the thickness of the embossed adhesive layer after embossing based on the same method as step (2), and determine whether the thickness of the adhesive in different areas meets the target adhesive thickness; if so, proceed to the next step, otherwise repeat step (5) until the thickness of the embossed adhesive layer after embossing meets the target adhesive thickness.

[0068] In more detail, after removing the working template 30, the thickness of each area of ​​the embossed adhesive layer after being acted upon by the working template is detected, and the detection position is the same as step (2), so that the detected area and the number of areas are the same, the thickness of each area is detected, and it is determined whether the thickness of each area meets the preset target glue thickness, and adjustments are made; in detail, when the thickness of each area meets the preset target glue thickness, step (7) is entered for the embossing process; when the thickness of each area does not meet the preset target glue thickness, step (5) is repeated to emboss the embossed adhesive layer with the working template, with the smooth surface of the working template facing the embossed adhesive layer; and the embossing is performed so that the distance between the working template and the substrate is the target glue thickness in step (3), and the operation is repeated in sequence until the thickness of each area detected meets the preset target glue thickness.

[0069] Of course, in the above step (6), when the thickness of each area does not meet the preset target glue thickness, step (5) is repeated, and based on the thickness of different areas, different areas can be appropriately selected to re-coat the embossed glue to perform the operation of step (5) again, so that the thickness of each area meets the preset target glue thickness.

[0070] After the above steps (1) to (6), a printed adhesive layer having a preset target adhesive thickness is obtained, and then the next step is performed.

[0071] Furthermore, in step (7), the imprinted adhesive layer in step (6) is imprinted based on a preset imprinting master 40, wherein the imprinting master 40 has a graphic structure to be imprinted and transferred; after curing, the imprinting master is removed to obtain a grating imprinting structure.

[0072] In this step, based on a preset imprint master 40, the imprint master has a patterned structure to be imprinted and transferred, such as a grating structure, including a coupling-in grating, a turning grating, a coupling-out grating and other micro-nano structures; Figure 6 As shown, the imprint master 40 is obtained by a semiconductor etching process, or by transfer, which is not the focus of the present invention, and can be obtained by a process in the prior art, and the present invention does not make any limitation. The imprint master 40 is applied along one side by roller pressing, thereby realizing the imprinting of the micro-nano structure.

[0073] Furthermore, in some other implementations, in step (1), it also includes plasma treatment of the surface of the substrate 10, and then providing a layer of adhesion promoter on the surface after the plasma treatment to increase the bonding force between the embossed adhesive and the substrate; and performing high-temperature heat treatment to form a stable chemical bond at the bonding interface; and then coating the embossed adhesive with a predetermined thickness and evenly distributing the adhesive.

[0074] In the present invention, through process steps (1) to (6), the thickness of the embossed adhesive layer in different areas is judged, the target thickness of the adhesive layer to be embossed is calculated by the thickness of the embossed adhesive layer in different areas, and the target thickness is realized and controlled by the surface-treated working template, thereby adjusting the thickness of the adhesive, thereby achieving uniformity control of the thickness; the problem of uneven thickness of the adhesive at high rotation speed can be improved, thereby improving the subsequent embossing process and improving the embossing quality.

[0075] Meanwhile, the present invention provides a diffractive optical waveguide, which is prepared based on the method provided by any of the above embodiments, and the thickness uniformity of the residual adhesive layer of the diffractive optical waveguide after embossing can be well controlled.

[0076] Through the process of the present invention, after improving the uniformity of the thickness of the glue, embossing is performed. After testing, the diffractive optical waveguide product obtained after embossing can greatly improve the uniformity of the thickness of the embossed residual glue, so that the thickness of the embossed residual glue layer in the middle area and other areas of the substrate surface is as consistent as possible, and the optical performance of the formed diffractive optical waveguide is improved, especially for the diffractive optical waveguide product formed in the middle part of the substrate, the optical performance is closer to that of the diffractive optical waveguides in other areas, so as to improve the quality of the entire embossing process and improve the qualified rate of the product.

[0077] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A grating imprinting method based on thickness adjustment, characterized in that: The steps include: (1) providing a substrate, coating a predetermined thickness of embossing adhesive on the surface of the substrate, and evenly coating the embossing adhesive to form an embossing adhesive layer; (2) detecting the thickness of the embossed adhesive layer after coating, and determining the thickness of the embossed adhesive layer in different areas; (3) determining a target coating thickness of the embossed adhesive layer according to the thickness of the embossed adhesive layer in different regions determined in step (2); (4) providing a working template, and performing surface treatment on any smooth surface of the working template so that the surface contact angle of the surface is greater than a preset value, thereby obtaining a smooth surface; (5) using the working template in step (4) to emboss the embossed adhesive layer, with the smooth surface of the working template facing the embossed adhesive layer; and performing embossing so that the distance between the working template and the substrate is equal to the target coating thickness in step (3); (6) removing the working template, and detecting the thickness of the embossed adhesive layer after embossing based on the same method as step (2), and judging whether the thickness of the adhesive layer in different regions meets the target adhesive layer thickness; if so, proceeding to the next step; otherwise, repeating step (5) until the thickness of the embossed adhesive layer after embossing meets the target adhesive layer thickness; (7) Based on a preset imprinting master, the imprinting adhesive layer in step (6) is imprinted, and the imprinting master has a graphic structure to be transferred by imprinting; after curing, the imprinting master is removed to obtain a grating imprinting structure.

2. A grating imprinting method based on thickness adjustment according to claim 1, characterized in that: In the step (1), before coating the embossing adhesive, the surface of the substrate is subjected to plasma treatment, and a layer of adhesion promoter is disposed on the surface after the plasma treatment.

3. A grating imprinting method based on thickness adjustment according to claim 1 or 2, characterized in that: In the step (2), at least the thickness of N regions of the embossed adhesive layer is detected, where N is greater than or equal to 3 and is a natural number.

4. The grating imprinting method based on thickness adjustment according to claim 3, characterized in that: In the step (3), based on the thickness H of the embossed adhesive layer in different regions N , determine the minimum value of the thickness of the plurality of embossed adhesive layers, and determine the target adhesive thickness H of the embossed adhesive layer based on the minimum value of the thickness of the embossed adhesive layer measured in different regions, H≥min(H1, H2, ... H N ).

5. The grating imprinting method based on thickness adjustment according to claim 3, characterized in that: The thickness H of the embossed rubber layer in different regions N , the target thickness H of the embossed adhesive layer is not greater than the average value of the thickness of the embossed adhesive layer in different regions, H≤(H1+H2......+H N ) / N.

6. A grating imprinting method based on thickness adjustment according to any one of claims 4 or 5, characterized in that: In the step (4), the surface contact angle is not less than 105°, so that the smooth surface has good hydrophobicity.

7. A grating imprinting method based on thickness adjustment according to any one of claims 4 or 5, characterized in that: The target coating thickness H is limited to a range of 30 nm to 300 nm.

8. A grating imprinting method based on thickness adjustment according to any one of claims 4 or 5, characterized in that: In step (5), force is uniformly applied to the working template so that the smooth surface of the working template acts uniformly on various areas of the embossed adhesive layer, so that the distance between the working template and the substrate is controlled to be the target adhesive thickness determined in the previous step.

9. A grating imprinting method based on thickness adjustment according to any one of claims 4 or 5, characterized in that: In step (6), when the thickness of each different area does not meet the preset target coating thickness, step (5) is repeated, and the process also includes selecting different areas to re-coat the embossed adhesive based on the thickness of the different areas to perform step (5) again.

10. A diffractive optical waveguide, characterized in that: The diffractive optical waveguide is prepared based on a grating imprinting method based on thickness adjustment as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Air pressure coating type nanoimprint lithography equipment and imprint lithography method

    CN111679553A

  • Manufacturing method of nanoimprint adhesive layer and optical element

    CN113900354A

  • Preparation method of microstructure

    CN117908323A

  • System and method for manufacturing press die for printing LCD oriented film

    CN1841165A

  • Offset printing machine and method for detecting defective roller nip width thereof

    JP2008194996A