Coke mechanical strength detection method based on image recognition

The particle size and area of ​​coke are calculated through image recognition technology, and the wear resistance and crushing resistance index is established, which solves the inaccuracy problem of coke mechanical strength detection in the existing technology, and realizes the quantitative description of coke mechanical properties and the blast furnace smelting process optimization.

CN118967660AActive Publication Date: 2024-11-15ANGANG STEEL CO LTD +1

Patent Information

Application Number
CN202411207404.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-15
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing metallurgical coke mechanical strength detection methods cannot accurately determine the coke particle size distribution and mechanical properties, resulting in a lack of representativeness and sensitivity of the detection results, which affects the optimization of the blast furnace smelting process.

Method used

Using image recognition-based detection method, by acquiring the images of coke samples, calculating the pixel diameter and area, establishing wear resistance index and crushing resistance index, and achieving a quantitative description of coke mechanical properties.

Benefits of technology

Improve the accuracy and speed of coke mechanical strength detection, provide detailed particle size distribution and average particle size data, solve the problems of poor representativeness and poor sensitivity of the detection results, and improve the quality of metallurgical coke and blast furnace smelting process. optimization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019410310000021
    Figure BDA0005019410310000021
  • Figure BDA0005019410310000022
    Figure BDA0005019410310000022
  • Figure BDA0005019410310000031
    Figure BDA0005019410310000031
Patent Text Reader

Abstract

The invention relates to a coke mechanical strength detection method based on image recognition, which comprises the following steps: acquiring an image of a coke sample, calculating and counting the total pixel diameter and the total number of the coke sample before and after the test, respectively counting each coke grain in the interval of 60-80mm and greater than 80m in the sample before the test, and calculating the average grain size to obtain 60-80mm and gt; the method comprises the following steps: calculating the average pixel particle size and the coke quantity of coke within the range of 10-20 mm, 20-40 mm, 40-60 mm, 60-80 mm and more than 80 mm after a sample test, calculating the average pixel particle size and the corresponding coke quantity of coke within the range of 10-20 mm, 20-40 mm, 40-60 mm, 60-80 mm and more than 80 mm after the sample test, calculating the coke pixel area proportion of each particle size range, establishing wear resistance indexes Ar1 to Ar3, establishing crush resistance indexes Rc1 to Rc2, and establishing a comprehensive mechanical strength index; the quantitative description of the mechanical property of the coke is realized, a manual screening and weighing method is replaced, and the problems that the representativeness of the mechanical strength of the coke is not strong, the sensitivity is poor, the granularity of the sampled coke affects the detection result and the like are solved while the detection speed is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ironmaking in the steel industry, and in particular to a method for detecting the mechanical strength of coke based on image recognition. Background Art

[0002] The mechanical strength of metallurgical coke determines its crushing performance and powder generation performance inside the blast furnace, and has a decisive impact on the air permeability of the entire material column of the blast furnace, the path and resistance of the rising gas flow. The current detection method of the mechanical strength of metallurgical coke is the method of manual screening and weighing using a rotary drum in the 1970s and 1980s. The mechanical properties are expressed by wear resistance M40 and crushing strength M10. M40 is the weight percentage of coke with a diameter greater than 40mm after the drum movement, and M10 is the weight percentage of coke with a diameter less than 10mm after the drum movement. This method can only roughly judge the deterioration behavior of coke after mechanical operation, and there are major drawbacks. The main problems are: 1. It is impossible to accurately determine the deterioration amount of coke after mechanical operation. For example, it is difficult to measure the actual particle size of coke less than 10mm. What is the diameter of coke with a particle size greater than 40mm after the drum movement, and how much has the actual particle size of coke decreased? 1. It is difficult to accurately describe the true mechanical properties of coke, and it is only possible to roughly judge whether the coke is "qualified"; 2. The sampling process has a significant impact on the test results. The method requires testing coke with a particle size greater than 60 mm, and then weighing the coke greater than 40 mm after the drum test. It is obvious that M40 will have a significant impact on the results when taking coke with a particle size of 80 mm and coke with a particle size of 60 mm; 3. The measurement results lack information on particle size distribution, and have poor guiding significance for blast furnaces and correspondence with the blast furnace smelting process. The blast furnace cannot adjust the smelting parameters and conduct detailed analysis through changes in M40 and M10. Summary of the invention

[0003] The present invention provides a method for detecting the mechanical strength of coke based on image recognition, which realizes the quantitative description of the mechanical properties of coke, replaces the original method of manual screening and weighing, improves the detection speed, and solves many problems such as the lack of representativeness of the mechanical strength of coke, poor sensitivity, and the influence of the sampled coke particle size on the detection result.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for detecting the mechanical strength of coke based on image recognition comprises the following steps:

[0006] S1. Obtain an image of a coke sample, measure the particle size of the coke before and after the drum test, and fill all the pixels into a square according to the number of pixels in the coke image, the side length of which is the pixel diameter of the coke;

[0007] S2. Calculate and count the total pixel diameter and total number of the coke sample before and after the test;

[0008] S3. Count each particle of coke in the range of 60-80 mm and greater than 80 mm in the sample before the test, and calculate the average particle size to obtain the average pixel particle size and the number of coke in the range of 60-80 mm and greater than 80 mm;

[0009] S4. Calculate the average pixel particle size and the corresponding coke quantity of the coke in the range of 10-20 mm, 20-40 mm, 40-60 mm, 60-80 mm and greater than 80 mm after the test of the sample;

[0010] S5, calculating the area ratio of coke pixels in each particle size interval;

[0011] S6. Establish wear resistance indexes Ar1 to Ar3, where Ar1 is the weight percentage of particles with a diameter less than 10 mm, Ar2 is the pixel area percentage of particles with a diameter in the range of 10 to 20 mm after the test, and Ar3 is the percentage increase in the total pixel area of ​​the coke before and after the test;

[0012] S7, establishing anti-crushing indexes Rc1 to Rc2;

[0013] Rc1 is the area ratio of pixels with particle size > 40 mm, which is the proportion of large particle size coke after mechanical movement of coke;

[0014] Rc2 is the percentage of coke fragmentation with a particle size of more than 80 mm, which is the proportion of coke fragmentation with large particle size after mechanical movement of coke;

[0015] S8. Establish a comprehensive mechanical strength index;

[0016] M1=(D-D') / D×100% (1)

[0017] Wherein, D is the average pixel size of coke before the sample test; D' is the average pixel size of coke after the sample test; M1 represents the reduction ratio of the average pixel size of coke after mechanical movement.

[0018] Furthermore, in step S1, the image of the coke sample is obtained by using a camera, and the camera is set at a distance of 0.2 to 5 m above the sample.

[0019] Furthermore, in step S2, the coke test is imaged and the particle size is calculated by the following formula:

[0020]

[0021] Among them, d is the pixel size of each coke particle in the coke test; S is the actual area of ​​the real area corresponding to the entire coke image; k is the number of pixels contained in the area of ​​each coke instance; HW is the total number of image pixels.

[0022] Furthermore, the calculation formula for the coke pixel area ratio in each particle size interval in step S5 is as follows:

[0023]

[0024] Among them, S i is the percentage of pixel area of ​​each size coke after the test; N' i is the number of cokes of each particle size after the test; N' is the total number of cokes after the test; i is the range of each particle size, with values ​​of 10, 20, 40, 60, 80, D' i The average pixel diameter of each coke particle size range after the test, the average pixel particle size of coke in the range of 10-20mm, 20-40mm, 40-60mm, 60-80mm and >80mm, is expressed as D' 10 , D' 20 , D' 40 , D' 60 , D' 80 .

[0025] Furthermore, in step S6,

[0026] Ar2=S' 10-20 =D' 10 2 ×N 10 / ∑(D' i 2 ×N' i )×100% (4)

[0027] Among them, S' 10-20 It is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test;

[0028]

[0029] Among them, D i is the average pixel diameter of each particle size range of coke before the test, N i is the amount of coke of each particle size before the test.

[0030] Furthermore, in step S7,

[0031] Rc1=S' 40-60 +S' 60-80 +S' >80 (6)

[0032] Among them, S'40-60 S' is the pixel area ratio of the coke particle size between 40 and 60 mm after the test; 60-80 S' is the pixel area ratio of the coke particle size between 60 and 80 mm after the test; >80 The percentage of pixel area of ​​coke with particle size greater than 80 mm after the test;

[0033] Rc2=(N 80 -N' 80 ) / N 80 ×100% (7)

[0034] Among them, N 80 N' is the number of coke particles with a particle size greater than 80 mm; 80 It is the average pixel particle size of coke with a particle size greater than 80 mm.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1) Use digital images to accurately measure the particle size of coke before and after the test, and use the concept of pixel area to quantify the particle size of each coke;

[0037] 2) Obtain detailed information on the particle size distribution, average particle size, coke quantity, coke pixel area change and other data before and after mechanical action. By establishing several wear resistance Ar index and anti-crushing Rc index based on image measurement, a quantitative description of the mechanical properties of coke can be achieved, replacing the original method of manual screening and weighing. While improving the detection speed, it also solves many problems such as the lack of representativeness of the mechanical strength of coke, poor sensitivity, and the influence of the sampled coke particle size on the detection results.

[0038] 3) It can be used to guide the advancement of coking technology and the establishment of new standards for blast furnace coke, greatly improving the quality of metallurgical coke and optimizing the blast furnace smelting process. DETAILED DESCRIPTION

[0039] The specific embodiments of the present invention are further described below:

[0040] The present invention provides a method for detecting the mechanical strength of coke based on image recognition, comprising the following steps:

[0041] S1. Obtain the image of the coke sample. The camera equipment is required to be 0.2 to 5m above the coke sample. The coke sample ensures that the paving edge is clear and there is no overlapping between the cokes. The coke sample has a particle size greater than 60mm and a weight of 50±0.2kg. The particle size of the coke before and after the drum test is measured using image recognition processing software. According to the number of pixels contained in the coke image, all pixels are filled into a square with a side length equal to the pixel diameter of the coke.

[0042] S2. Use image processing software to calculate the particle size of the coke test in an image format to obtain the pixel particle size d of each particle of coke in the coke test: Use the DeblurGANv2 algorithm to deblur the obtained coke image; Use the labelme tool to label the clear coke image, and perform data enhancement on the labeled coke image to obtain the coke image dataset required for training; By combining the coco dataset and the coke image dataset, train the improved MaskRCNN model to obtain the instance segmentation model for coke target detection; After deblurring the coke image collected in real time, use the trained instance segmentation model to perform detection, and obtain the number of cokes N in the coke image and the corresponding actual area of ​​coke according to the detection results; Use the coke area calculation formula to calculate the corresponding coke pixel particle size from the actual area of ​​coke obtained by formula 1;

[0043] The calculation formula for the pixel size of each coke particle is:

[0044]

[0045] Wherein, d is the pixel size of each particle of coke in the coke test; S is the actual area of ​​the real area corresponding to the entire coke image; k is the number of pixels contained in the area of ​​each coke instance; HW is the total number of image pixels; the actual physical meaning of the pixel size of coke is: fill the projection area of ​​coke on the plane with the side length of a solid square area, the pixel size of coke is ≤ the diameter of the sieve hole that coke can pass through, and the pixel size of each particle of coke in the sample is averaged to obtain d, which is recorded as the average pixel size D of coke in this batch of samples.

[0046] S3. Count each particle of coke in the sample with a particle size of 60 to 80 mm and larger than 80 mm and calculate the average particle size to obtain D 60 , D 80 , respectively, represent the average pixel size of coke between 60 and 80 mm and larger than 80 mm, in mm, N 60 、N 80 They respectively represent the number of cokes in the range of 60-80mm and larger than 80mm in the sample, in pieces.

[0047] S4. Take out the sample after the drum test. The drum test includes ASTM drum test, JIS drum test, Mikum drum test, ISO drum IRSID drum test, GB / T2006-94 Chinese national standard drum test, and GB / T2006-80 Chinese national standard drum test.

[0048] S5. The sample after step 4 is sieved with a sieve with a mesh of 10 mm, and the image particle size detection is performed on the sieve according to steps S1 to S3, and the total number of cokes in the sample N', the average pixel diameter of coke D', and the average pixel particle size D' of coke in the range of 10-20 mm, 20-40 mm, 40-60 mm, 60-80 mm and greater than 80 mm are obtained respectively. 10 , D' 20 , D' 40 , D' 60 , D' 80 , and the corresponding coke quantity N' 10 、N' 20 、N' 40 、N' 60 、N' 80 .

[0049] S6. Calculate the coke pixel area ratio S in each particle size range according to the following formula i , use S i Indicates the particle size distribution of coke after mechanical action.

[0050]

[0051] Among them, S i is the percentage of pixel area of ​​each size coke after the test; N' i is the number of cokes of each particle size after the test, in pieces; N i is the total amount of coke after the test, in pieces; i is the range of each particle size, with values ​​of 10, 20, 40, 60, and 80, D' i The average pixel diameter of each coke particle size range after the test, the average pixel particle size of coke in the range of 10-20mm, 20-40mm, 40-60mm, 60-80mm and >80mm, is expressed as D' 10 , D' 20 , D' 40 , D' 60 , D' 80 , unit: mm.

[0052] S7, establish wear resistance indexes Ar1 to Ar3 respectively,

[0053] Ar1 is the weight percentage of particles with a diameter less than 10 mm, indicating the weight of powder produced by coke;

[0054] Ar2 is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test, indicating the degree to which the coke produces small particle size coke;

[0055] Ar2=S' 10-20 =D' 10 2 ×N10 / ∑(D' i 2 ×N' i )×100% (10)

[0056] Among them, S' 10-20 It is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test;

[0057] Ar3 is the percentage increase of the total pixel area of ​​coke before and after the test, indicating the percentage increase of the overall pixel area of ​​coke after mechanical movement, reflecting the degree of coke breakage after mechanical movement;

[0058]

[0059] Among them, D i is the average pixel diameter of each particle size range of coke before the test, N i is the amount of coke of each particle size before the test.

[0060] S8, establishing anti-crushing indexes Rc1 to Rc2;

[0061] Rc1 is the area ratio of pixels with particle size > 40 mm, which is the proportion of large particle size coke after mechanical movement of coke;

[0062] Rc1=S' 40-60 +S' 60-80 +S' >80 (11)

[0063] Among them, S' 40-60 is the pixel area ratio of the coke particle size in the range of 40 to 60 mm after the test; S' 60-80 S' is the pixel area ratio of the coke particle size in the range of 60 to 80 mm after the test; >80 The percentage of pixel area of ​​coke with particle size greater than 80 mm after the test;

[0064] Rc2 is the percentage of coke fragmentation with a particle size of more than 80 mm, which is the proportion of coke fragmentation with large particle size after mechanical movement of coke;

[0065] Rc2=(N 80 -N' 80 ) / N 80 ×100% (12)

[0066] Among them, N 80 N' is the number of coke particles with a particle size greater than 80 mm; 80 It is the average pixel particle size of coke in the range greater than 80 mm.

[0067] S9. Establish a comprehensive mechanical strength index:

[0068] M1=(D-D') / D×100% (13)

[0069] M1 represents the percentage of reduction in the average pixel particle size of coke after mechanical movement. It can comprehensively reflect the degradation properties of coke in the blast furnace and is a comprehensive manifestation of wear resistance and anti-breakage performance. Its value is equal to the percentage of reduction in the average particle size of coke after mechanical action, that is, the degree of reduction in the coke particle size. The average particle size of coke after wear and beating can be directly calculated through this value. The smaller the value, the smaller the degree of reduction in the average particle size of coke after wear and beating, and the higher the strength of the coke.

[0070] The following examples are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples. The methods used in the following examples are conventional methods unless otherwise specified.

[0071] [Example]

[0072] S1. Select coke with a particle size greater than 60 mm and a weight of 50 ± 0.2 kg, and obtain an image of the coke sample to ensure that the tiling edges are clear and there is no overlapping between the cokes.

[0073] S2. Use image processing software to calculate the particle size of the coke test image to obtain the pixel size d of each particle of coke in the coke test.

[0074] The calculation formula for the pixel size of each coke particle is:

[0075]

[0076] Among them, d is the pixel size of each particle of coke in the coke test; S is the actual area of ​​the actual area corresponding to the entire coke image; k is the number of pixels contained in the area of ​​each coke instance; HW is the total number of image pixels; the actual physical meaning of the pixel size of coke is: fill the projection area of ​​coke on the plane with the side length of a solid square area, the pixel size of coke ≤ the diameter of the sieve hole that coke can pass through, and the pixel size of each particle of coke in the sample is averaged to obtain d, which is recorded as the average pixel size D of coke in this batch of samples.

[0077] S3. Count each particle of coke in the sample with a particle size of 60 to 80 mm and larger than 80 mm and calculate the average particle size to obtain D 60 , D 80 , respectively, represent the average pixel size of coke between 60 and 80 mm and larger than 80 mm, in mm, N 60 、N 80 They represent the number of cokes in the range of 60-80 mm and larger than 80 mm in the sample, in units of pieces; the specific measurement data are shown in Table 1.

[0078] Table 1

[0079] <![CDATA[D 60(mm) ]]> 68.4 <![CDATA[N 60(个) ]]> 82 <![CDATA[D 80(mm) ]]> 86.6 <![CDATA[N 80(个) ]]> 36 <![CDATA[D (mm) ]]> 74.0 <![CDATA[N (个) ]]> 118

[0080] S4. Take out the sample after subjecting it to the Chinese national standard drum test GB / T2006-80.

[0081] S5. Perform image particle size detection on the material on the sieve. Obtain the total number of coke samples N', the average pixel diameter of coke D', and the average pixel particle diameter D' of coke in the range of 10-20mm, 20-40mm, 40-60mm, 60-80mm and greater than 80mm. 10 , D' 20 , D' 40 , D' 60 , D' 80 , and the corresponding coke quantity N' 10 、N' 20 、N' 40 、N' 60 、N' 80 .

[0082] S6. Calculate the coke pixel area ratio S in each particle size range according to the following formula i , use S i Indicates the particle size distribution of coke after mechanical action.

[0083]

[0084] The specific measurement and calculation data are shown in Table 2.

[0085] Table 2

[0086]

[0087]

[0088] S7. Expression of wear resistance index: establish wear resistance index Ar1 to Ar3 respectively.

[0089] Ar1 is the weight percentage of particles with a diameter less than 10 mm, indicating the weight of powder produced by coke;

[0090] Ar2 is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test, indicating the degree to which the coke produces small particle size coke;

[0091] Ar2=S' 10-20 =D' 10 2 ×N 10 / ∑(D' i 2 ×N'i )×100=14.4 2 ×201 / (867800)*100=4.8% (16)

[0092] Among them, S' 10-20 It is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test;

[0093] Ar3 is the percentage increase of the total pixel area of ​​coke before and after the test, indicating the percentage increase of the overall pixel area of ​​coke after mechanical movement, reflecting the degree of coke breakage after mechanical movement;

[0094]

[0095] S8, the expression of the anti-crushing index, and the establishment of the anti-crushing indexes Rc1 to Rc2 respectively;

[0096] Rc1 is the pixel area ratio of particle size>40mm,

[0097] Rc1=S' 40-60 +S' 40-60 +S' >80 =(313124+341718+82867) / 867800×100%=85.0%(18)

[0098] It indicates the proportion of coke with large particle size after mechanical movement of coke;

[0099] Rc2 is the percentage of coke fragments with a particle size of more than 80 mm.

[0100] Rc2=(N 80 -N' 80 ) / N 80 ×100=(36-12) / 36×100%=66.67%; (19)

[0101] It indicates the proportion of large-size coke that breaks after mechanical movement.

[0102] S9. Establish a comprehensive mechanical strength index

[0103] M1=(D-D') / D×100=(74.0-35.2) / 74.0×100%=52.43% (20)

[0104] It indicates the percentage of reduction in the average pixel particle size of coke after mechanical movement, which can comprehensively reflect the degradation properties of coke in the blast furnace and is a comprehensive manifestation of wear resistance and anti-breakage performance. Its value is equal to the percentage of reduction in the average particle size of coke after mechanical action, that is, the degree of reduction in the coke particle size. The average particle size of coke after wear and beating can be directly calculated through this value. The smaller the value, the smaller the degree of reduction in the average particle size of coke after wear and beating, and the higher the strength of the coke.

Claims

1. A method for detecting the mechanical strength of coke based on image recognition, characterized in that: The steps include: S1. Obtain an image of a coke sample, measure the particle size of the coke before and after the drum test, and fill all the pixels into a square according to the number of pixels in the coke image, the side length of which is the pixel diameter of the coke; S2. Calculate and count the total pixel diameter and total number of the coke sample before and after the test; S3. Count each particle of coke in the range of 60-80 mm and larger than 80 mm in the sample before the test, and calculate the average particle size to obtain the average pixel particle size and the number of coke in the range of 60-80 mm and larger than 80 mm; S4. Calculate the average pixel particle size and the corresponding coke quantity of the coke in the range of 10-20 mm, 20-40 mm, 40-60 mm, 60-80 mm and greater than 80 mm after the test of the sample; S5, calculating the area ratio of coke pixels in each particle size interval; S6. Establish wear resistance indexes Ar1 to Ar3, where Ar1 is the weight percentage of particles with a diameter less than 10 mm, Ar2 is the pixel area percentage of particles with a diameter in the range of 10 to 20 mm after the test, and Ar3 is the percentage increase in the total pixel area of ​​the coke before and after the test; S7, establishing anti-crushing indexes Rc1 to Rc2; Rc1 is the area ratio of pixels with particle size > 40 mm, which is the proportion of large particle size coke after mechanical movement of coke; Rc2 is the percentage of fragmented coke with a particle size of more than 80 mm, which is the proportion of coke with large particle size that is fragmented after mechanical movement of coke; S8. Establish a comprehensive mechanical strength index; M1=(D-D') / D×100% (1) Wherein, D is the average pixel size of coke before the sample test; D' is the average pixel size of coke after the sample test; M1 represents the reduction ratio of the average pixel size of coke after mechanical movement.

2. A coke mechanical strength detection method based on image recognition according to claim 1, characterized in that: In the step S1, an image of the coke sample is obtained by using a camera, and the camera is set at a distance of 0.2 to 5 m above the sample.

3. The method for detecting the mechanical strength of coke based on image recognition according to claim 1, characterized in that: In step S2, the coke test is imaged and the particle size is calculated by the following formula: Among them, d is the pixel size of each coke particle in the coke test; S is the actual area of ​​the real area corresponding to the entire coke image; k is the number of pixels contained in the area of ​​each coke instance; HW is the total number of image pixels.

4. The method for detecting the mechanical strength of coke based on image recognition according to claim 1, characterized in that: The calculation formula for the coke pixel area ratio in each particle size interval in step S5 is as follows: Among them, S i is the percentage of pixel area of ​​each size coke after the test; N' i is the number of cokes of each particle size after the test; N' is the total number of cokes after the test; i is the range of each particle size, with values ​​of 10, 20, 40, 60, 80, D' i The average pixel diameter of each coke particle size range after the test, the average pixel particle size of coke in the range of 10-20mm, 20-40mm, 40-60mm, 60-80mm and >80mm, is expressed as D' 10 , D' 20 , D' 40 , D' 60 , D' 80 .

5. The method for detecting the mechanical strength of coke based on image recognition according to claim 1, characterized in that: In step S6, Among them, S' 10-20 It is the pixel area ratio of the coke particle size in the range of 10 to 20 mm after the test; Among them, D i is the average pixel diameter of each particle size range of coke before the test, N i is the amount of coke of each particle size before the test.

6. The method for detecting the mechanical strength of coke based on image recognition according to claim 1, characterized in that: In step S7, Rc1=S' 40-60 +S' 60-80 +S' >80 (6) Among them, S' 40-60 is the pixel area ratio of the coke particle size in the range of 40 to 60 mm after the test; S' 60-80 is the pixel area ratio of the coke particle size in the range of 60 to 80 mm after the test; S' >80 The percentage of pixel area of ​​coke with particle size greater than 80 mm after the test; Rc2=(N 80 -N' 80 ) / N 80 ×100% (7) Among them, N 80 N' is the number of coke particles with a particle size greater than 80 mm; 80 It is the average pixel particle size of coke with a particle size greater than 80 mm.

Citation Information

Patent Citations

  • Method for automatically detecting aeolotropism in charred coal organization

    CN101097205A

  • Coke granularity identification detection method and detection system

    CN116051512A

  • Measuring method of coke strength, estimating method of coke strength, and producing method of coke

    JP2020158642A

  • Method for predicting average particle size of coke

    JP2021165340A

Cited By

  • Method for quantitatively predicting coke lumpiness by matching lean coal in coking coal

    CN120800937A