Deacidification reinforcing agent as well as preparation method and application thereof
By coating and modifying nano calcium carbonate, nano-CaCO3/SiO2 complex is prepared with ethyl cellulose and diphenyl isooctyl phosphate to form a deacidification reinforcement, which solves the deacidification treatment in the prior art The problems of reduced durability and shortened film life have achieved effective prevention and treatment of cellulose acetate films and extended life.
Patent Information
- Application Number
- CN202410960781.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
AI Technical Summary
The existing deacidification treatment methods have reduced durability and shortened film life of cellulose acetate films, especially in severe acidification environments, and the prior art is difficult to effectively prevent and treat acetic acid syndrome.
The nano-CaCO3/SiO2 composite was prepared by inorganic substances to combine nano-CaCO3/SiO2 composite with ethyl cellulose and diphenyl isooctyl phosphate to form a deacidification reinforcement, improve deacidification performance and enhance the film hydrophobicity.
It extends the durability of the deacid reinforcement and the life of the film, improves the preservation ability in an acidic environment, prevents and treats acetic acid syndrome, enhances the hydrophobicity of the film, and reduces the occurrence of catalytic degradation reactions.
Smart Images

Figure CN118969113A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of image protection and relates to a deacidification strengthening agent and a preparation method and application thereof. Background Art
[0002] Photographic images carry a wealth of archival information and are a valuable legacy in the modern history of mankind. Films with cellulose acetate as the base material are widely used photosensitive materials since the 1950s. Due to the characteristics of the base material, the instability of the temperature and humidity of the storage environment, and the airtight collection packaging, most cellulose acetate films will develop a disease called "acetic acid syndrome" over time. After the occurrence of acetic acid syndrome, the film base material undergoes a hydrolysis reaction, and the reaction formula is: ROAc+H2O→HOAc+ROH. A large amount of acetic acid is released during the reaction. Conversely, the acetic acid environment will continue to catalyze the occurrence of the hydrolysis reaction. As cellulose acetate continues to degrade, the mechanical strength of the film decreases, it distorts and deforms, and the image is polluted, causing the film to lose its value.
[0003] There are many existing treatment methods for the "acetic acid syndrome" film that secretes plasticizer pollutants, twists and deforms. For example, researchers have proposed the potential of using tea and tea waste as adsorbents, and evaluated their adsorption capacity by the adsorption effects of acetic acid, water, and plasticizer dibutyl phthalate (DBP). The results show that although tea and tea waste are not as effective as commercial adsorbents on the market, they are low-cost and widely available, and have further research value and significance. Other researchers have used sodium carbonate and sodium polyacrylate (SPA) as deacidifiers and dehumidifiers for experiments, and used high-performance liquid chromatography (HPLC) to quantitatively evaluate the deacidification of sodium carbonate. The results show that the performance of sodium carbonate is better than that of commercial deacidifiers; SPA can control the relative humidity in the container at about 40%, and has a good dehumidification effect. The two materials are feasible for the prevention and treatment of "acetic acid syndrome".
[0004] In existing research, the study of acetic acid syndrome of movie films can also be prevented by controlling the storage environment. It is known that sub-zero low temperature environment cannot effectively prevent the occurrence of acetic acid syndrome. Although the movie film body can be repaired and protected for the film that has been twisted, deformed, and hardened into blocks in the later stage, the nature of cellulose acetate will still undergo hydrolysis and release acetic acid gas. Therefore, it is necessary to deacidify and reinforce the film body to achieve the purpose of long-term preservation.
[0005] A Chinese patent document with reference application number CN202310516318.4 discloses a method for in-situ formation of calcium carbonate in paper documents and a deacidification process. The method for in-situ formation of calcium carbonate in paper documents is obtained by reacting calcium hydroxide with carbon dioxide; the method for deacidification of acidified paper documents is: preparation of a water-soluble cellulose derivative solution, preparation of a calcium hydroxide dispersion, and pressure atomization treatment of the acidified paper documents; carbon dioxide treatment, in-situ generation of calcium carbonate and vacuum drying treatment, balancing the moisture in a constant temperature and humidity chamber to complete the treatment.
[0006] Although the existing deacidification treatment method has a significant deacidification effect, it is mainly used for the deacidification of paper documents and cannot be applied to the deacidification of film with a serious acetic acid content (pH ≤ 4). At the same time, during deacidification, the acidified paper documents need to be immersed in a compound deacidification solution, which will reduce the durability of the deacidification solution and shorten the life of the film. Summary of the invention
[0007] In view of the technical problems of reduced durability of deacidification liquid and shortened film life in existing deacidification, the present invention provides a deacidification reinforcing agent and a preparation method and application thereof.
[0008] The invention utilizes inorganic substances to coat and modify nano calcium carbonate, and the obtained product is compounded with ethyl cellulose, diphenyl isooctyl phosphate and an organic solvent to obtain a deacidification reinforcing agent, which can improve the deacidification performance and the hydrophobicity of the film, thereby extending the durability of the deacidification reinforcing agent and the life of the film.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] A deacidification reinforcing agent comprises the following raw materials in weight fractions: 3% to 7% ethyl cellulose, 1.5% to 2% nano-CaCO3 / SiO2 compound and 0.1% to 0.5% diphenyl isooctyl phosphate, and the rest is an organic solvent.
[0011] It is further defined that the deacidification reinforcing agent comprises the following raw materials in weight fractions: 6.7% ethyl cellulose, 2% nano-CaCO3 / SiO2 composite and 0.5% diphenyl isooctyl phosphate, and the rest is an organic solvent.
[0012] It is further defined that the nano-CaCO3 / SiO2 composite is obtained by using sodium silicate and nano-calcium carbonate as raw materials through a countercurrent method; in the composite, the mass ratio of silicon dioxide to nano-calcium carbonate is 6% to 10%.
[0013] It is further limited that the organic solvent is n-butanol, banana water, ethyl acetate, tetraethyl orthosilicate or acetone solution.
[0014] It is further defined that the asymmetric stretching vibration peak of the Si—O—Si bond in the nano-CaCO3 / SiO2 composite is 1105.25 cm -1 Redshifted to 1090.1 cm -1 , the Si—O bond bending vibration peak changes from 805.47 cm -1 Redshifted to 800.8 cm -1 Place.
[0015] The preparation method of the deacidification reinforcing agent as described comprises the following steps:
[0016] S1. Weigh sodium silicate and nano calcium carbonate respectively according to the mass ratio, and prepare nano-CaCO3 / SiO2 composite by countercurrent method;
[0017] S2. Add ethyl cellulose to the organic solvent according to the mass ratio, then add the nano-CaCO3 / SiO2 composite of step S1, and finally add diphenyl isooctyl phosphate, and mix well to obtain a suspension, which is the deacidification reinforcing agent.
[0018] It is further defined that the preparation process of step S1 is specifically:
[0019] Take nano calcium carbonate solid and water, prepare a suspension with a solid content of 10%, stir evenly and set aside;
[0020] The suspension is heated to 80°C to 90°C, and sodium silicate is added; then 4 ml of a 20% mass concentration dilute sulfuric acid solution is added dropwise at a rate of 2 ml / min. After the addition is completed, the suspension is kept warm, and the nano-CaCO3 / SiO2 composite is obtained by stirring, settling, filtering, washing and drying.
[0021] It is further defined that the stirring speed is 450 r / min to 500 r / min, the stirring time is 40 min to 60 min, and the sedimentation time is 20 h to 24 h.
[0022] It is further defined that in step S2, the conditions for uniform mixing are: stirring at 300 r / min to 400 r / min for 40 min to 60 min, and ultrasonic dispersion for 2 h to 4 h.
[0023] The use of the deacidification consolidating agent in preventing film acetic acid syndrome.
[0024] The beneficial effects of the present invention are:
[0025] 1. The deacidification reinforcing agent provided by the present invention can improve the deacidification performance while also improving the hydrophobicity of the film, thereby extending the durability of the deacidification reinforcing agent and the life of the film, and is used for the prevention and treatment of film acetic acid syndrome.
[0026] 2. The nano-CaCO3 / SiO2 composite material used as the raw material of the deacidification reinforcement agent of the present invention is obtained by coating and modifying nano-calcium carbonate with inorganic substances. The modification of nano-calcium carbonate by coating can eliminate the high surface potential energy of nano-calcium carbonate and improve the binding force with the organic polymer base material, thereby enhancing the dispersibility and acid resistance of nano-calcium carbonate in oily media and improving the deacidification effect of the deacidification reinforcement agent.
[0027] 3. When the present invention uses sodium silicate to coat nano-calcium carbonate, the mass ratio of sodium silicate to silicon dioxide is 1:10. At this time, the coated SiO2 is more and can coat CaCO3. The surface of the composite has both the excellent properties of nanoparticles and changes the surface characteristics of ultrafine particles, thereby increasing the shelf life of the film in an acidic environment.
[0028] 4. The deacidification strengthening agent provided by the present invention is hydrophobic, and the hydrophobicity is improved after film formation, so that the film is not easily attacked by water molecules, reducing the occurrence of catalytic degradation reactions of the film, thereby extending the life of the film.
[0029] 5. The deacidification reinforcing agent provided by the present invention has better hydrophobicity in a hot and humid environment and can protect severely acidified cellulose acetate film. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the effect of the proportion [m(SiO2) / m(CaCO3)] on the acid resistance of the composite;
[0031] Figure 2 IR spectra of CaCO3 and SiO2;
[0032] Figure 3 is the IR spectrum of CaCO3 / SiO2 composite;
[0033] Figure 4 XRD patterns of CaCO3 and CaCO3 / SiO2 composites;
[0034] Figure 5 Deacidification strengthening agents prepared for different organic solvents and their film formation on the film surface;
[0035] Figure 6 The scanning electron microscope images of the film before and after coating, where: a is sample 1; b is sample 2; c is sample 3; d is sample 4; e is sample 5;
[0036] Figure 7 This is the surface element distribution diagram of sample 2 after coating;
[0037] Figure 8 This is the surface element distribution map of sample 5 after coating;
[0038] Fig. 9 The surface contact angle results of sample 1; where: a is 30s; b is 60s; c is 120s;
[0039] Fig.10 The surface contact angle results of sample 2; where: a is 30s; b is 60s; c is 120s;
[0040] Fig.11 The surface contact angle results of sample 3; where: a is 30s; b is 60s; c is 120s;
[0041] Fig.12 The surface contact angle results of sample 4; where: a is 30s; b is 60s; c is 120s;
[0042] Fig.13 The surface contact angle results of sample 5; where: a is 30s; b is 60s; c is 120s;
[0043] Fig.14 It is the folding endurance of the film before and after coating;
[0044] Fig.15 It is the tensile strength of the film before and after coating;
[0045] Fig.16 It is the transmittance spectrum of the base layer of different film samples;
[0046] Fig.17 It is the reflectance spectrum of the base layer of different film samples;
[0047] Fig.18 It is the tensile strength of the film after 28 days of acetic acid aging. DETAILED DESCRIPTION
[0048] The technical solution protected by the present invention is now described in detail in conjunction with the accompanying drawings and embodiments. However, it is obvious that the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the described embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0049] The deacidification reinforcing agent provided by the invention comprises the following raw materials in weight fractions: 3% to 7% ethyl cellulose, 1.5% to 2% nano-CaCO3 / SiO2 compound and 0.1% to 0.5% diphenyl isooctyl phosphate (DPOP), and the rest is organic solvent.
[0050] Preferably, the mass fraction of ethyl cellulose is 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 6.7% or 7%. The mass fraction of nano-CaCO3 / SiO2 composite is 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2%; the mass fraction of DPOP is 0.1%, 0.2%, 0.3%, 0.4% or 0.5%.
[0051] It is further defined that the deacidification strengthening agent comprises the following raw materials in weight fractions: 6.7% ethyl cellulose, 2% nano-CaCO3 / SiO2 composite and 0.5% diphenyl isooctyl phosphate (DPOP), and the rest is organic solvent.
[0052] In the present invention, the nano-CaCO3 / SiO2 composite is obtained by using sodium silicate and nano-calcium carbonate as raw materials through a countercurrent method; in the nano-CaCO3 / SiO2 composite, the mass ratio of silicon dioxide to nano-calcium carbonate is 6% to 10%.
[0053] The organic solvent used in the present invention is n-butanol, banana water, ethyl acetate, ethyl orthosilicate or acetone solution.
[0054] The present invention also provides a method for preparing a deacidification reinforcing agent, comprising the following steps:
[0055] S1. Sodium silicate and nano calcium carbonate are weighed respectively according to the above mass ratio, and a nano-CaCO3 / SiO2 composite is prepared by a countercurrent method.
[0056] The specific preparation process of this step is: take nano calcium carbonate solid and water, prepare a suspension with a solid content of 10%, stir evenly for use; heat the suspension to 80℃~90℃, and then add sodium silicate; then add 4ml of dilute sulfuric acid solution with a mass concentration of 20% at a rate of 2ml / min, keep warm after the addition is completed, stir, settle, filter, wash and dry to obtain nano-CaCO3 / SiO2 composite.
[0057] In this step, the reaction formula of sodium silicate and sulfuric acid is as follows: Na2SiO3+H2SO4=H2SiO3+Na2SO4, the generated H2SiO3 decomposes into SiO2 and H2O at high temperature (80℃~90℃); and then forms nano-CaCO3 / SiO2 complex with nano calcium carbonate.
[0058] In the present invention, the stirring speed is 450 r / min to 500 r / min, the stirring time is 40 min to 60 min, and the sedimentation time is 20 h to 24 h.
[0059] Preferably, the stirring speed is 450 r / min, 460 r / min, 470 r / min, 480 r / min, 490 r / min or 500 r / min; the stirring time is 40 min, 45 min, 50 min, 55 min or 60 min; and the sedimentation time is 20 h, 21 h, 22 h, 23 h or 24 h.
[0060] S2. Add ethyl cellulose to the organic solvent according to the above mass ratio, then add the nano-CaCO3 / SiO2 composite of step S1, and finally add diphenyl isooctyl phosphate DPOP, and mix well to obtain a suspension, which is the deacidification reinforcing agent.
[0061] In step S2 of the present invention, the conditions for uniform mixing are: stirring at a speed of 300 r / min to 400 r / min for 40 min to 60 min, and ultrasonic dispersion for 2 h to 4 h.
[0062] Preferably, the rotation speed is 300 r / min, 320 r / min, 350 r / min, 380 r / min or 400 r / min; the time is 40 min, 45 min, 50 min, 55 min or 60 min; and the ultrasonic dispersion is 2 h, 2.5 h, 3 h, 3.5 h or 4 h.
[0063] The deacidification reinforcement agent provided by the invention uses inorganic substances to coat nano calcium carbonate, and the formed composite can improve the dispersibility and acid resistance of the nano calcium carbonate in oily media; ethyl cellulose (EC) has good film-forming property, and when mixed with n-butanol solution, the solution has good leveling property, fast film-forming speed, good adhesion and good hydrophobicity, and forms a smooth protective film with a dense mesh and a thickness of 50-100 μm on the surface of the film after drying, so that the deacidification reinforcement agent has a good preventive effect on film acetic acid syndrome.
[0064] The present invention is described in detail below with reference to specific embodiments.
[0065] It should be noted that, unless otherwise specified, the reagents and drugs used in the following examples and experiments are conventional commercially available products.
[0066] It should be noted that, unless otherwise specified, the operations used in the following examples and experiments are routine operations in the art.
[0067] Example 1
[0068] The purpose of this embodiment is to use inorganic substances to coat nano calcium carbonate, and the resulting composite can improve the dispersibility and acid resistance of nano calcium carbonate in oily media. This is because: inorganic electrolytes adsorbed on the surface of calcium carbonate particles can, on the one hand, increase the ion surface potential, induce steric hindrance effect, produce double-layer electrostatic repulsion, and promote the dispersion and refinement of agglomerated particles, reduce their surface energy, increase the contact angle, and make their surface lipophilic; on the other hand, the steric hindrance effect prevents hydrogen ions from contacting the inner layer of calcium carbonate particles, thereby improving the acid resistance of nano calcium carbonate.
[0069] Preferably, in this embodiment, sodium silicate and nano calcium carbonate are used as raw materials, and SiO2 is coated on the surface of nano CaCO3 by a countercurrent method under certain conditions to prepare a nano-CaCO3 / SiO2 composite.
[0070] The nano-CaCO3 / SiO2 composite provided in this embodiment is prepared as follows:
[0071] (1) taking nano calcium carbonate (solid) and adding ultrapure water to prepare a suspension with a solid content of 10%, stirring evenly for later use;
[0072] (2) The suspension was heated in a water bath at 90° C., sodium silicate was added, and then 4 ml of a 20% sulfuric acid solution was added dropwise at a rate of 2 ml / min. After the addition was completed, the suspension was kept warm and stirred at a speed of 450 r / min for 1 h. The suspension was then allowed to settle for 24 h. The suspension was filtered, washed three times, and dried to obtain a silica-coated nano-calcium carbonate composite, i.e., a nano-CaCO3 / SiO2 composite.
[0073] Utilize SiO2 to coat nano-CaCO3, [m(SiO2) / m(CaCO3)] batching ratio can affect SiO2 to CaCO3 coating situation, in order to measure SiO2 coating ratio to CaCO3 / SiO2 influence of compound acid resistance.Present embodiment respectively presses m(SiO2) / m(CaCO3) batching ratio 6%, 8%, 10% and 12%, drops sodium silicate in nano-calcium carbonate slurry, other conditions are unchanged.After reaction is finished, ageing 24h, pickling time is taken 0.5h, 10h and 24h.
[0074] Determination of Ca in the CaCO3 / SiO2 composite acid leaching solution prepared with different ingredient ratios by EDTA titration 2+ Concentration, the results are as follows Figure 1 shown.
[0075] When m(SiO2) / m(CaCO3)=6%, the generated SiO2 cannot cover CaCO3, and the compounding ratio is increased. It is found that the composite soaking liquid Ca 2+When the concentration decreases, when m(SiO2) / m(CaCO3)=10%, c(Ca 2+ )
[0076] =0.020mol / L, at this time, the amount of coated SiO2 is large. Continue to increase the amount of m(SiO2), c(Ca 2+ ) increases, indicating that the local concentration of SiO2 increases, self-agglomeration occurs, and the generated SiO2 single substance is not coated on CaCO3. According to the experimental results, the batching ratio m(SiO2) / m(CaCO3)=10% is selected.
[0077] In this embodiment, the performance of the nano-CaCO3 / SiO2 composite prepared when the ratio of m(SiO2) / m(CaCO3)=10% was tested.
[0078] 1. Infrared spectrum test
[0079] A PE-Frontier Fourier infrared spectrometer was used in the wavelength range of 450 cm -1 ~4000cm -1 Under the conditions of , three samples of nano-CaCO3 / SiO2 composite, nano-CaCO3 and nano-SiO2 were tested by infrared spectroscopy. The test results are as follows Figure 2 and Figure 3 shown.
[0080] from Figure 2 It can be seen that: 1790cm -1 、1456.6cm -1 、872.39cm -1 、710.68cm -1 is the characteristic peak position of CaCO3, where 1790cm -1 The peak at 1456.6 cm is the vibration peak of the C=O bond of CaCO3. -1 CO3 in CaCO3 2- Characteristic absorption peak; 1630.58cm -1 、1105.25cm -1 、805.47cm -1 is the characteristic peak position of SiO2, where 1105.25cm -1 The peak of asymmetric stretching vibration of Si—O—Si bond is 805.47 cm -1 The peak is the Si—O bond bending vibration peak.
[0081] from Figure 3It can be seen that in the infrared spectrum of the nano-CaCO3 / SiO2 composite, the characteristic absorption peaks of CaCO3 and SiO2 appear at the same time, and the characteristic peak of SiO2 red-shifts, and the asymmetric stretching vibration peak of the Si—O—Si bond shifts from 1105.25 cm -1 Redshifted to 1090.1 cm -1 , the Si—O bond bending vibration peak changes from 805.47 cm -1 Redshifted to 800.8 cm -1 This indicates that there is silicon dioxide in the nano-CaCO3 / SiO2 composite after coating and that silicon dioxide reacts chemically with calcium carbonate to form a bond.
[0082] 2. X-ray diffraction test
[0083] The nano-CaCO3 / SiO2 composite and nano-CaCO3 samples were tested by X-ray diffraction using a SmartLab (9) high-resolution X-ray diffractometer at a scanning angle of 2θ = 10° to 60° and a step angle of 0.05° / step. The XRD patterns of CaCO3 and CaCO3 / SiO2 composite are shown in Figure 4 shown.
[0084] from Figure 4 It can be seen that: after coating with SiO2, the crystal plane spacing and position of the CaCO3 diffraction peak are almost the same, but the intensity of the diffraction peak is significantly reduced, indicating that the generated SiO2 is coated on the CaCO3 surface in an amorphous structure, producing a shielding effect.
[0085] According to the Debye-Scherrer formula:
[0086]
[0087] D: grain size;
[0088] K: Scherrer constant, taken as 0.89;
[0089] λ: X-ray wavelength, 0.15406nm;
[0090] β: half-height width of the sample diffraction peak;
[0091] θ: diffraction angle.
[0092] According to the above formula, the grain size of uncoated CaCO3 is about 28.31nm, and the grain size of coated CaCO3 / SiO2 composite is about 29.38nm, and the grain size is still less than 30nm. It can be seen that the particle performance will not be affected by the size change.
[0093] In summary, in this embodiment, sodium silicate (silicon dioxide) is used to coat nano calcium carbonate. The surface of the composite not only has the excellent properties of nano particles, but also changes the surface characteristics of ultrafine particles. The formed composite can improve the dispersibility and acid resistance of nano calcium carbonate in oily media, so as to increase the shelf life of the film in an acidic environment.
[0094] Example 2
[0095] The deacidification reinforcement agent provided in this embodiment includes the following raw materials in mass fractions: 6.7% ethyl cellulose, 2% nano-CaCO3 and 0.5% DPOP, and the rest is an organic solvent.
[0096] In this embodiment, the nano-CaCO3 / SiO2 composite is prepared when the proportion of m(SiO2) / m(CaCO3)=10%.
[0097] In this embodiment, the organic solvent is selected as n-butanol solution.
[0098] In this embodiment, the preparation method of the deacidification reinforcement agent is:
[0099] Ethyl cellulose (EC) and an organic solvent are mixed, and then dry nano-CaCO3 / SiO2 powder is added into the system. After high-speed stirring for 1 hour, ultrasonic dispersion is performed for 2 hours to allow the nano-CaCO3 / SiO2 particles to be grafted with the hydroxyl groups on the surface of EC to form a stable EC / nano-CaCO3 / SiO2 network composite structure. DPOP is then added to enhance the stability of the solution system, and finally a suspension is obtained, which is the deacidification reinforcement agent.
[0100] Embodiment 3 to Embodiment 6
[0101] Different from Example 2, the organic solvents used in the deacidification reinforcement agents in Examples 3 to 7 are banana water, ethyl acetate, tetraethyl orthosilicate and acetone solution, respectively, and deacidification reinforcement agents with four different organic solvents are prepared accordingly.
[0102] The deacidification reinforcement agents prepared from different organic solvents in Examples 2 to 6 were evenly coated on the surface of the cleaned cellulose acetate film, and after drying, the surface drying time, leveling, film appearance, and sedimentation were compared. The results are shown in Tables 1 and Figure 5 shown.
[0103] Table 1 Solvent screening for deacidification materials
[0104] Solvents Dry time Leveling Appearance Settlement situation (72h) n-Butanol 80s excellent Smooth and smooth, no brush marks No trace of sediment Banana water 60s excellent Grainy, with brush marks Microprecipitation Ethyl acetate 60s Difference Slight coating marks, grainy feel Sedimentation Tetraethyl orthosilicate 80s excellent Slight coating marks, grainy feel Sedimentation acetone 60s Difference Severe brush marks, high whiteness Microprecipitation
[0105] From Table 1 and Figure 5It can be seen that: when banana water is used as a solvent, although the leveling property is good, the surface granularity is heavy, which affects the original picture information; when ethyl acetate and tetraethyl orthosilicate are used as solvents, the solution has obvious sedimentation and 3-5mm stratification; when acetone is used as a solvent, the leveling property of the solution is poor, the brush marks are obvious, and the picture is increased after film formation. When n-butanol is used as an organic solvent, the leveling property is good, the film is smooth and the dispersion is good, and the original picture information can be maintained. It can be seen that ethyl cellulose (EC) has good film-forming properties. When blended with n-butanol solution, the solution has good leveling properties, fast film formation speed, good adhesion, and good hydrophobicity. After drying, a dense mesh with a thickness of 50μm-100μm is formed on the film surface. Smooth protective film.
[0106] In Example 2 of the present invention, the mass fraction of ethyl cellulose can be any other value within the range of 3% to 7%; the mass fraction of nano-CaCO3 / SiO2 composite can be any other value within the range of 1.5% to 2%; the mass fraction of DPOP can be any other value within the range of 0.1% to 0.5%.
[0107] In order to verify the effect of the deacidification reinforcement agent provided by the present invention on the prevention and treatment of acetic acid syndrome film, the following test was carried out using the deacidification reinforcement agent prepared in Example 2; at the same time, the following comparative example was set in the test.
[0108] Comparative Example 1
[0109] The deacidification reinforcing agent provided in this comparative example includes: 80% n-butanol solution, 6.7% ethyl cellulose, 2% nano-CaCO3 and 0.5% DPOP.
[0110] The preparation method of this comparative example refers to Example 2.
[0111] Comparative Example 2
[0112] The deacidification reinforcing agent provided in this comparative example includes: 70% WPU, 0.5% OP-10 and 5% nano-CaCO3.
[0113] The preparation method of this comparative example refers to Example 2.
[0114] Comparative Example 3
[0115] The deacidification reinforcing agent provided in this comparative example includes: 80% n-butanol solution, 6.7% ethyl cellulose, 1.5% nano-CaCO3, 0.5% SiO2, and 0.5% DPOP.
[0116] The preparation method of this comparative example refers to Example 2.
[0117] Experiment 1: Effects of different deacidification and strengthening agents on film surface morphology
[0118] Test samples: deacidification reinforcement prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3
[0119] Test method: Take five cellulose triacetate films of the same size and having "acetic acid syndrome" (pH≤4), one of which is not coated with any deacidification reinforcing agent (referred to as sample one); the remaining four films are coated with the deacidification reinforcing agent of Example 2 (referred to as sample two), the deacidification reinforcing agent of Comparative Example 1 (referred to as sample three), the deacidification reinforcing agent of Comparative Example 2 (referred to as sample four) and the deacidification reinforcing agent of Comparative Example 3 (referred to as sample five).
[0120] (1) Scanning electron microscope test
[0121] The above samples 1, 2, 3, 4 and 5 were cut into 1 cm × 1 cm samples to be tested, fixed on the scanning electron microscope sample stage with conductive glue, and gold was sprayed for 120 seconds using an SCD005 ion sputtering instrument to enhance conductivity. The surface morphology of the film was observed using a SU3500 tungsten filament scanning electron microscope at an acceleration voltage of 3 kV and a magnification of 1000 times, and the results are shown in Figure 6.
[0122] from Figure 6 It can be seen that the surface of the acetate film base with acetic acid syndrome has a lot of depressions, protrusions and scratches; the surface of sample 2, sample 3, sample 4 and sample 5 is smooth after coating, indicating that the composite deacidification material can eliminate these defects. Sample 3 and sample 4 still have a small amount of scratches, while sample 2 and sample 5 introduce nano-SiO2, which can effectively eliminate scratches and reduce the impact on the film image.
[0123] (2) EDS test
[0124] This test is mainly to analyze the types and distribution of elements on the film surface. Take the above sample 2 and sample 5 for EDS test. The EDS result of sample 2 is shown in 7, and the EDS result of sample 5 is shown in 8.
[0125] from Figure 7 and Figure 8 It can be seen that on the surface of sample 2, the three main elements of Ca, O, and Si are evenly distributed within the scanning range. The distribution positions of silicon and calcium are similar, and the silicon element is evenly distributed, indicating that the Namo-CaCO3 / SiO2 complex is evenly dispersed in the solution and evenly distributed on the film surface after coating. The Ca and Si elements on the surface of sample 5 are locally aggregated and unevenly distributed, indicating that the electrostatic adsorption effect between the same nanoparticles is large when they are directly physically mixed, and they are prone to aggregate to form larger particles, affecting the optical and physical properties of the film.
[0126] It can be seen that the element distribution of using namo-CaCO3 / SiO2 composite as deacidification material is more uniform than directly blending nano-CaCO3 and nano-SiO2 as deacidification material, indicating that the deacidification performance of the deacidification reinforcement agent can be improved by coating.
[0127] Test 2: Effect of deacidification and strengthening agent on the physical properties of film
[0128] Test samples: deacidification reinforcement agents prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3.
[0129] Test method: Take five cellulose triacetate films of the same size and having "acetic acid syndrome", one of which is not coated with any deacidification reinforcing agent (referred to as sample one); the remaining four films are coated with the deacidification reinforcing agent of Example 2 (referred to as sample two), the deacidification reinforcing agent of Comparative Example 1 (referred to as sample three), the deacidification reinforcing agent of Comparative Example 2 (referred to as sample four) and the deacidification reinforcing agent of Comparative Example 3 (referred to as sample five).
[0130] (1) Contact angle
[0131] Take the five sample films mentioned above, cut 1cm×1cm samples to be tested and paste them on a glass slide, use DSA100 optical contact angle meter to measure the contact angle of the film substrate surface under the condition of 2μL droplet volume, the test results are shown in Figures 9 to 13 .
[0132] Fig. 9 The contact angle changes of the substrate surface of sample 1 at 30s, 60s and 120s. It can be seen that the contact angle decreases from 64.7° to 39.8°, with a decrease rate of 38.5%. Fig.10 The contact angle changes of the substrate surface of sample 2 at 30s, 60s and 120s. The contact angle decreases from 95.1° to 91.3°, with a decrease rate of 3.9%. Fig.11 The contact angle of sample 3 at 30s, 60s, and 120s decreased from 89.0° to 79.2°, with a decrease rate of 11.0%. Fig.12 The contact angle of sample 4 at 30s, 60s, and 120s decreased from 95.0° to 57.9°, with a decrease rate of 39.0%. Fig.13 The contact angle of sample 5 at 30s, 60s, and 120s decreased from 83.0° to 74.9°, with a decrease rate of 9.8%.
[0133] By comparison, it can be seen that the deacidification reinforcement agent prepared in Example 2 has the slowest contact angle decrease rate, indicating that the deacidification reinforcement agent prepared in the present invention is hydrophobic and the hydrophobicity is improved after film formation, making the film less susceptible to attack by water molecules, reducing the occurrence of film catalytic degradation reactions, thereby extending the life of the film.
[0134] (2) Folding endurance and tensile strength
[0135] According to GB / T 9858-2009 “Determination of folding resistance of film base and film”, the film to be tested is balanced at a temperature of 23±3℃ and a relative humidity of 30%-50% for 72 hours, and the film is cut into 15mm×120mm test samples with a paper cutter. The number of reciprocating folds is measured using an LB-MIT135 paper folding tester under the conditions of a tension of 4.91N and an angle of 135°±2°.
[0136] According to GB / T12683-2009 "Determination of tensile properties of film base and film", the film to be tested is balanced at a temperature of 23±3℃ and a relative humidity of 30% to 50% for 72 hours, and the film is cut into 15mm×180mm test samples with a paper cutter. The sample is clamped vertically between two chucks, and its tensile strength is measured using a Kc-136pc universal material testing machine at a gauge length of 10cm and a tensile speed of 20mm / min, and the tensile strength of the sample is calculated.
[0137] The calculation formula for the sample tensile strength is:
[0138]
[0139] Where: F is the average tensile strength (N); b is the width of the specimen (mm).
[0140] Take the above five sample films and test them respectively using the above method. The folding endurance results of each film are as follows: Fig.14 The tensile strength results of each film are shown in Fig.15 shown.
[0141] See also Fig.14 and Fig.15It can be seen that the folding resistance and tensile strength of the acetate film after coating are improved. Compared with the uncoated sample, the folding resistance of sample 2 is increased by 25% and the tensile strength is increased by 22%. This is because the EC / nano-CaCO3 / SiO2 composite material fills the surface gaps of the film and improves the folding resistance of the film. Compared with pure nano-CaCO3, the modified nano-CaCO3 / SiO2 is combined with EC. The interface viscosity between the composite particles and the matrix is enhanced, which is conducive to the transmission of stress and can improve the tensile strength to a certain extent. The deacidified material in sample three and sample four is single-element nano-CaCO3, which has high particle surface energy and is prone to "agglomeration" in the solution, preventing the movement of polymer chains. Although the tensile properties of the film are improved compared to when it is not coated, the improvement is limited. Although sample five adds nano-SiO2, nano-SiO2 and nano-CaCO3 are directly mixed and no bonding reaction is formed, so the properties of nano-CaCO3 itself are not changed. In addition, the dispersed and agglomerated particles will also affect the network structure of the composite material on stress transfer. The folding endurance and tensile strength have no obvious changes compared to sample three.
[0142] Test 3: Film optical properties
[0143] This test is mainly to compare the transmittance and reflectivity of the film with different deacidification strengthening agents.
[0144] The test method is: take five films of the same size and which have developed "acetic acid syndrome", remove the film emulsion layer with a diluted sodium hypochlorite solution (water: sodium hypochlorite = 1:1), dry the film base and cut it into a suitable size. Then, no deacidification reinforcing agent is applied to one of the films (referred to as sample 1); the deacidification reinforcing agent of Example 2 (referred to as sample 2), the deacidification reinforcing agent of Comparative Example 1 (referred to as sample 3), the deacidification reinforcing agent of Comparative Example 2 (referred to as sample 4), and the deacidification reinforcing agent of Comparative Example 3 (referred to as sample 5) are applied to the remaining four films.
[0145] Samples 1, 2, 3, 4 and 5 were taken, and the transmittance and reflectance of the treated samples were tested using a UV-Lambda950 ultraviolet near-infrared spectrophotometer at a wavelength range of 350 nm to 750 nm and a scanning rate of 300 nm / min.
[0146] The relationship between transmittance and reflectivity can be expressed by the following formula:
[0147] α+ρ+τ=1
[0148] Where: α is the absorptivity, ρ is the reflectivity, and τ is the absorptivity.
[0149] The test results of transmittance and reflectance are shown in Table 2. Fig.16 and Fig.17 shown.
[0150] Table 2 Comparison of transmittance and reflectance
[0151] Sample name Light transmittance Reflectivity Sample 1 93.1%~76.6% 6.6%~12.0% Sample 2 95.0%~82.4% 3.8%~6.9% Sample 3 93.9%~79.5% 4.5%~7.8% Sample 4 93.0%~78.2% 5.0%~8.5% Sample 5 93.3%~77.8% 5.0%~8.2%
[0152] from Fig.16 , Fig.17 As can be seen from Table 2, the transmittance of sample 2 is the highest at 93.9% to 79.5%, and the reflectivity is the lowest at 3.8% to 6.9%. This indicates that the EC / nano-CaCO3 / SiO2 composite deacidified material prepared in this experiment has a better effect on filling film base scratches, reducing surface roughness, and reducing light scattering and reflection.
[0153] Test 4: Deacidification and aging test
[0154] Before the test, five cellulose triacetate films of the same size and having developed "acetic acid syndrome" were taken, one of which was not coated with any deacidification reinforcing agent (referred to as sample one); the remaining four films were coated with the deacidification reinforcing agent of Example 2 (referred to as sample two), the deacidification reinforcing agent of Comparative Example 1 (referred to as sample three), the deacidification reinforcing agent of Comparative Example 2 (referred to as sample four), and the deacidification reinforcing agent of Comparative Example 3 (referred to as sample five).
[0155] (1) Effect of different deacidification materials on film acidity (pH)
[0156] In order to further verify the protective effect of the composite deacidification material on acetate film, acetic acid aging and wet heat aging were performed on Sample 1, Sample 2, Sample 3, Sample 4 and Sample 5, respectively, and the acidity (pH) of the film at different aging times was measured.
[0157] Acetic acid aging experiment: 10g of glacial acetic acid was placed in a vacuum desiccator with a volume of about 5.5L. After 24 hours of volatilization, the acetic acid gas concentration was about 1g / L and the humidity was 65%. The sample was then placed in a sealed container and aged for 28 days.
[0158] Hygrothermal aging test: Each sample was placed in an HCP hygrothermal aging chamber, and the temperature was set at 50°C and the relative humidity was 70%. The aging time was 28 days.
[0159] pH determination: Select different sample films, cut them into 1mm×1mm squares, weigh 1.00±0.01g of the film to be tested and put it into a wide-mouth bottle, add 100mL of ultrapure water, slowly stir in a water bath at 38±1℃ for 24h, filter and take a small amount of solution, and use S210pH meter to determine its acidity. The test results are shown in Table 3.
[0160] Table 3 Changes in acidity before and after film coating
[0161]
[0162]
[0163] As can be seen from Table 3, without any reinforcement film protection, the acidity of sample 1 decreased from 3.97 and 4.03 to 3.42 and 3.44, with a decrease rate of 13.9% and 14.6%; among the samples that were deacidified and reinforced, sample 2 had the most significant deacidification effect, with pH values reaching 6.45 and 6.62, reaching the safe pH range, and after aging, it decreased to 5.96 and 6.21, with decrease rates of 5.6% and 6.2% respectively; the decrease rates of sample 3 were 10.8% and 11.4%; the decrease rates of sample 4 were 7.8% and 7.6%; the decrease rates of sample 5 were 9.3% and 10.7%.
[0164] At the same time, the deacidification effect and durability were compared, sample 2> sample 3> sample 5> sample 4, indicating that the deacidification and reinforcement effect of EC / nano-CaCO3 / SiO2 composite material on pH≤4 film is better than EC / namo-CaCO3 composite deacidification material and WPU / nano-CaCO3 composite deacidification material. It is further verified that the acid resistance of nano-CaCO3 / SiO2 composite material is better than the blending effect of nano-CaCO3 and nano-SiO2, and the hydrophobicity is better in a hot and humid environment, which can protect severely acidified cellulose acetate film.
[0165] (2) Tensile strength
[0166] The test method is the same as that in Test 2 for folding endurance and tensile strength.
[0167] The tensile strength of the film was tested after 28 days of acetic acid aging. The line graph is as follows Fig.18 shown.
[0168] See also Fig.18 After 28 days of acetic acid aging, the tensile strength of the film continued to decrease. The tensile strength of sample 1 decreased from 15.74 kN / m to 11.24 kN / m, with a decrease rate of 28.6%, while the decrease rates of samples 2, 3, 4 and 5 were 17.6%, 20.6%, 19.8% and 17.7% respectively. With the degradation and aging of cellulose triacetate, the β-glycosidic bonds between D-pyranose groups break, the molecular structure of the polymer is destroyed, and the molecular chains are arranged horizontally along the cellulose, linked by hydrogen bonds, which is manifested as a decrease in tensile strength.
[0169] Compared with samples 3 and 4, after the deacidification agent of sample 2 forms a film, the hydroxyl (-OH) on the surface of the coated and modified nano-CaCO3 / SiO2 particles can bond with the ethyl group in the EC long chain to form a hydroxyethyl group, which has good stability; therefore, the tensile strength of sample 2 after coating is the largest and the rate of decline after aging is the lowest. Although silica is also added to the deacidification agent used in sample 5, it is not evenly distributed in the skeleton pores of ethyl cellulose with CaCO3, and the bonding formed is limited. The macromolecular agglomeration hinders the reorganization of the cellulose acetate molecular chain and cannot effectively improve the tensile strength of the film.
[0170] In the present invention, when the mass fraction of the raw materials in the deacidification reinforcing agent is changed to form deacidification reinforcing agents of different proportions, the above method is used to verify the performance, and it is found that it exhibits the same or similar performance as the deacidification reinforcing agent in Example 2. Therefore, the deacidification reinforcing agent provided by the present invention has hydrophobicity and good deacidification reinforcing performance, and prolongs the storage time of triacetate cellulose film with severe "acetic acid syndrome" after deacidification treatment.
[0171] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A deacidification reinforcing agent, characterized in that: The deacidification reinforcing agent comprises the following raw materials in weight fractions: 3% to 7% ethyl cellulose, 1.5% to 2% nano-CaCO3 / SiO2 compound and 0.1% to 0.5% diphenyl isooctyl phosphate, and the rest is organic solvent.
2. The deacidification reinforcing agent according to claim 1, characterized in that The deacidification reinforcing agent comprises the following raw materials in weight fractions: 6.7% ethyl cellulose, 2% nano-CaCO3 / SiO2 composite and 0.5% diphenyl isooctyl phosphate, and the rest is organic solvent.
3. The deacidification reinforcing agent according to claim 1, characterized in that The nano-CaCO3 / SiO2 composite is obtained by using sodium silicate and nano-calcium carbonate as raw materials through a countercurrent method; in the composite, the mass ratio of silicon dioxide to nano-calcium carbonate is 6% to 10%.
4. The deacidification reinforcing agent according to claim 1, characterized in that The organic solvent is n-butanol, banana water, ethyl acetate, tetraethyl orthosilicate or acetone solution.
5. The deacidification reinforcing agent according to claim 1, characterized in that The asymmetric stretching vibration peak of Si—O—Si bond in the nano-CaCO3 / SiO2 composite is 1105.25 cm -1 Redshifted to 1090.1 cm -1 , the Si—O bond bending vibration peak changes from 805.47 cm -1 Redshifted to 800.8 cm -1 Place.
6. The method for preparing the deacidification reinforcing agent according to claim 4, characterized in that: The preparation method comprises the following steps: S1. Weigh sodium silicate and nano calcium carbonate respectively according to the mass ratio, and prepare nano-CaCO3 / SiO2 composite by countercurrent method; S2. Add ethyl cellulose to the organic solvent according to the mass ratio, then add the nano-CaCO3 / SiO2 composite of step S1, and finally add diphenyl isooctyl phosphate, and mix well to obtain a suspension, which is the deacidification reinforcing agent.
7. The preparation method according to claim 6, characterized in that: The preparation process of step S1 is specifically as follows: Take nano calcium carbonate solid and water, prepare a suspension with a solid content of 10%, stir evenly and set aside; The suspension is heated to 80°C to 90°C, and sodium silicate is added; then 4 ml of a 20% mass concentration dilute sulfuric acid solution is added dropwise at a rate of 2 ml / min. After the addition is completed, the suspension is kept warm, and the nano-CaCO3 / SiO2 composite is obtained by stirring, settling, filtering, washing and drying.
8. The preparation method according to claim 7, characterized in that: The stirring speed is 450r / min~500r / min, the stirring time is 40min~60min, and the sedimentation time is 20h~24h.
9. The preparation method according to claim 6, characterized in that: In step S2, the conditions for uniform mixing are: stirring at 300 r / min to 400 r / min for 40 min to 60 min, and ultrasonic dispersion for 2 h to 4 h.
10. Use of the deacidification strengthening agent as claimed in claim 1 in preventing film acetic acid syndrome.
Citation Information
Cited By
Physical reutilization of siliconized papers
US20250034805A1