Wireless charging magnetic core and preparation method and application thereof
By splicing multiple sub-cores with insulating materials and using CNC processing, the eddy current loss and heat dissipation problems of large-scale, high-power wireless charging magnetic cores are solved, and efficient and uniform core performance is achieved.
Patent Information
- Application Number
- CN202411134027.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
Smart Images

Figure CN118969460A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of magnetic materials, and in particular to a wireless charging magnetic core and a preparation method and application thereof. Background Art
[0002] The national standard GB / T 38775.1-2020 for wireless charging systems for electric vehicles stipulates that the technical requirements for wireless charging (power transmission) equipment use frequencies of 19-21kHz and 79-90kHz; the rated transmission power requirements for equipment operating in the 19-21kHz frequency band are greater than 22kW, but should be less than 120kW; for equipment operating in the 79-90kHz frequency band, the rated transmission power should be less than 22kW. The transmission power of the transformer is positively correlated with the frequency and the cross-sectional area of the core, and negatively correlated with the number of turns of the primary coil. Therefore, high-power transformers in the 19-21kHz and 79-90kHz frequency bands require large-sized manganese-zinc power ferrite cores. In order to improve charging efficiency, the cross-sectional area of the core is usually 500cm 2 above.
[0003] Manganese-zinc power ferrite cores are usually prepared by powder molding combined with high-temperature sintering process. The molding pressure is proportional to the cross-sectional area of the core (F = K*Ae, K = 2.5 ~ 3.0T / cm 2 ), the cross-sectional area of the core is generally not more than 100cm 2 Therefore, it is impossible to use a direct molding process to prepare the above-mentioned large-scale ferrite core for wireless charging.
[0004] CN206649977U utility model patent, the utility model uses 6 fan-shaped magnetic cores to splice into a cylinder and fix them with a fixing sleeve at the middle through hole. However, this solution is only suitable for the preparation of simple magnetic cores, and cannot prepare complex and large-sized magnetic cores (such as pot-shaped, E-shaped, etc.).
[0005] The invention patent CN113990614A discloses a distributed air-gap planar transformer, which belongs to the field of switching power supply transformer design, including two discrete magnetic core I rods, a discrete magnetic core middle column, two discrete magnetic core side columns, and 6 air gaps between the discrete magnetic core side columns (middle column) and the discrete magnetic core I rod, and the size of the air gap is controlled by a thermal conductive glue with porcelain beads. The planar transformer of the invention has 6 air gaps evenly distributed, mainly to reduce local heating of the winding, reduce eddy current loss of the magnetic core, etc. However, the process provided by the prior art is only applicable to small-sized planar transformer cores, whose cross-sectional area is generally <100cm 2 , the power does not exceed 0.5kW and cannot be used in high-power wireless charging systems.
[0006] Therefore, providing a wireless charging magnetic core that can have the advantages of a large cross-sectional area and a high charging power while also ensuring that the eddy current loss of the wireless charging magnetic core is low and the heat dissipation uniformity during operation is an issue that needs to be urgently addressed. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a wireless charging magnetic core and its preparation method and application. The wireless charging magnetic core in the present invention has the advantages of large cross-sectional area and high charging power. At the same time, the sub-magnetic cores in the wireless charging magnetic core are separated by an insulating layer, so that the eddy current loss of the wireless charging magnetic core is small and the heat dissipation uniformity is good during operation.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a wireless charging magnetic core, the wireless charging magnetic core comprising a chassis magnetic core, an inner ring magnetic core and an outer ring magnetic core located on the surface of the chassis magnetic core, and the cross-sectional area of the wireless charging magnetic core is 500cm 2 In the above, the chassis magnetic core, the inner ring magnetic core and the outer ring magnetic core each include at least two sub-magnetic cores and an insulating layer located between the sub-magnetic cores.
[0010] In the wireless charging magnetic core provided by the present invention, the chassis magnetic core, the inner ring magnetic core and the outer ring magnetic core jointly construct a specific magnetic circuit, so that the charging coil generates a directional magnetic field or receives a directional magnetic field when working.
[0011] The wireless charging magnetic core provided by the present invention has a large cross-sectional area and can carry a power of more than 20kW; at the same time, the sub-magnetic cores of each component in the magnetic core provided by the present invention are separated by an insulating layer, which can reduce eddy current losses during charging and improve the uniformity of heat dissipation during operation.
[0012] Preferably, the inner ring magnetic core is located in a middle area on the surface of the chassis magnetic core.
[0013] The "middle area" mentioned in the present invention refers to the area within the edge area in the horizontal direction of the surface of the chassis magnetic core.
[0014] Preferably, there is a spacing area in the inner ring magnetic core.
[0015] Preferably, the outer ring magnetic core is located in an edge area on the surface of the chassis magnetic core.
[0016] Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core.
[0017] Preferably, there is a spacing area in the outer ring magnetic core.
[0018] Preferably, there is a distance between the outer ring magnetic core and the inner ring magnetic core.
[0019] Preferably, the center of the chassis core has a hole.
[0020] The present invention does not limit the size of the hole in the center of the chassis magnetic core, and those skilled in the art can select it according to needs.
[0021] Preferably, the charging power of the wireless charging magnetic core is 20-60 kW, that is, the rated power is 20-60 kW, for example, 20 kW, 25 kW, 30 kW, 35 kW, 40 kW, 45 kW, 50 kW, 55 kW or 60 kW.
[0022] Preferably, the structure of the inner ring magnetic core includes any one of a square ring, a circular ring, a racetrack type or a concave-convex structure, or a combination of at least two of them.
[0023] Preferably, the structure of the outer ring magnetic core includes any one of a square ring, a circular ring or a concave-convex structure, or a combination of at least two of them.
[0024] In a second aspect, the present invention provides a method for preparing the wireless charging magnetic core as described in the first aspect, the preparation method comprising:
[0025] The sub-magnetic cores are spliced into a chassis magnetic core and an inner ring magnetic core and an outer ring magnetic core located on the surface of the chassis magnetic core through insulating materials to obtain the wireless charging magnetic core.
[0026] The present invention realizes the splicing of sub-cores in the wireless charging magnetic core through insulating materials, and combines the precise positioning control of the sub-cores during the splicing process to prepare a wireless charging magnetic core with a large cross-sectional area and high power; and the sub-cores are separated by insulating materials, which effectively reduces the eddy current loss of the wireless charging magnetic core and improves its heat dissipation uniformity during operation.
[0027] Preferably, the shape of the cross section of the sub-core includes any one of square, rectangle, arc, ring, trapezoid, L-shape or concave-convex shape, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of square and rectangle, a combination of square and arc, a combination of rectangle and arc, a combination of rectangle and trapezoid, a combination of rectangle and L-shape, a combination of square and trapezoid, a combination of square and L-shape, a combination of trapezoid and concave-convex shape, a combination of arc and L-shape, or a combination of rectangle, square and concave-convex shape, etc.
[0028] Preferably, the side length of the square is 50-120 mm, for example, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 105 mm, 110 mm, 115 mm or 120 mm.
[0029] Preferably, the length of the rectangle is 50-150 mm, for example, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 120 mm, 130 mm, 140 mm or 150 mm.
[0030] Preferably, the width of the rectangle is 5 to 120 mm, for example, 5 mm, 10 mm, 15 mm, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm or 120 mm.
[0031] Preferably, the included angle of the arc is 0 to 180° and does not include 0°, for example, 1°, 3°, 5°, 7°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, 90°, 100°, 120°, 140°, 160° or 180°, etc.
[0032] Preferably, the outer diameter of the arc or ring is independently selected from 150 to 600 mm, for example, 150 mm, 180 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, 450 mm, 500 mm, 550 mm or 600 mm.
[0033] Preferably, the inner diameter of the arc or ring is independently selected from 50 to 550 mm, for example, 50 mm, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, 450 mm, 500 mm or 550 mm.
[0034] Preferably, the length of the first side of the L-shape is 50-150 mm, for example, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm or 150 mm.
[0035] Preferably, the width of the L-shaped first side is 20-50 mm, for example, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm or 50 mm.
[0036] In the present invention, the "length of the first side of the L-shape" can be found in Figure 6 The "width of the first side of the L-shape" can be found in paragraph a1 of Figure 6Paragraph a2 in .
[0037] Preferably, the length of the second side of the L-shape is 50-150 mm, for example, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm or 150 mm.
[0038] Preferably, the width of the second side of the L-shape is 20-50 mm, for example, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm or 50 mm.
[0039] In the present invention, the "second side length of the L-shape" can be found in Figure 6 The "width of the second side of the L-shaped part" can be found in paragraph b1 of Figure 6 Section b2 in .
[0040] Preferably, the first side and the second side of the L-shape are transitioned by a rounded corner.
[0041] Preferably, the cross-sectional shape of the sub-core in the vertical direction includes any one of square, rectangle, arc, ring, trapezoid, L-shape or concave-convex shape, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of rectangle and concave-convex shape, a combination of square and concave-convex shape, a combination of L-shape and concave-convex shape, a combination of trapezoid and concave-convex shape, a combination of square and arc, a combination of rectangle and arc, a combination of rectangle and trapezoid, a combination of rectangle and L-shape, a combination of square and L-shape, a combination of arc and L-shape, or a combination of rectangle, square and concave-convex shape, etc.
[0042] In the present invention, the "concave-convex shape" refers to a shape that is convex in the middle and concave on both sides, or a shape that is concave in the middle and convex on both sides, or a shape in which the concave area is located at one side edge of the overall concave-convex shape.
[0043] Preferably, in the concavo-convex shape, the length corresponding to the convex area is greater than the length corresponding to the concave area.
[0044] In the present invention, a concave-convex shape is selected in the cross-sectional shape of the sub-magnetic core in the vertical direction for splicing, and an outer ring magnetic core or an inner ring magnetic core with a spacing area can be formed by designing the splicing process.
[0045] The present invention does not limit the thickness of the sub-core in the vertical direction, and those skilled in the art can select it as needed.
[0046] Preferably, the sub-magnetic core includes a first sub-magnetic core, a second sub-magnetic core and a third sub-magnetic core.
[0047] Preferably, the first sub-magnetic cores are spliced to form a first splicing assembly for preparing a chassis magnetic core.
[0048] Preferably, the second sub-magnetic cores are spliced to form a second splicing assembly for preparing an inner ring magnetic core.
[0049] Preferably, the third sub-magnetic cores are spliced to form a third splicing assembly for preparing an outer ring magnetic core.
[0050] Preferably, the first sub-core, the second sub-core and the third sub-core all comprise manganese-zinc power ferrite cores.
[0051] Optionally, the sub-core used in the present invention can be a commercially available manganese-zinc power ferrite core or a manganese-zinc power ferrite core prepared by powder molding combined with nitrogen protection sintering process, and those skilled in the art can make the selection as needed.
[0052] Preferably, the insulating material is insulating glue.
[0053] The present invention uses insulating glue to splice the sub-magnetic cores, so that the sub-magnetic cores in the obtained wireless charging magnetic core are separated by the insulating layer formed by the insulating glue, which can further reduce the eddy current loss of the wireless charging magnetic core and further improve the heat dissipation uniformity during operation.
[0054] Preferably, the insulating glue includes any one of epoxy resin, AB glue or polyurethane glue.
[0055] In the present invention, the types of insulating materials used to prepare the chassis magnetic core, the outer ring magnetic core and the inner ring magnetic core can be the same or different.
[0056] Preferably, the specific preparation process of the chassis magnetic core includes: using the insulating material to bond the side surfaces of the first sub-magnetic core to each other to form a first splicing assembly, and after a first heating, obtaining the chassis magnetic core.
[0057] Preferably, the side surface of the first sub-magnetic core needs to be ground before being coated with the insulating material.
[0058] Preferably, the first heating temperature is 100-180°C, for example, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C, etc.
[0059] In the present invention, if the first heating temperature is too high, the cooling time required after the magnetic core is solidified is too long; if the first heating temperature is too low, the adhesive force of the glue is insufficient.
[0060] Preferably, the first heating time is 60 to 180 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0061] The preparation method of the present invention uses insulating materials to perform a splicing process on the sub-magnetic cores, and then performs a heat treatment to achieve sufficient solidification of the insulating material during the splicing process of the sub-magnetic cores. The splicing process of the insulating material is combined with the heating process of the insulating material to achieve effective splicing between the magnetic cores, which is conducive to the preparation of a wireless charging magnetic core with excellent performance, a large cross-sectional area and high charging power.
[0062] Preferably, before preparing the chassis magnetic core, the first heated material is further subjected to grinding and cutting processing.
[0063] The present invention performs fine processing on the obtained chassis magnetic core through grinding and cutting processes, and can obtain a chassis magnetic core with any structure and meeting the dimensional accuracy requirements, so that the preparation method of the present invention has the advantages of high processing accuracy and small dimensional tolerance.
[0064] As a preferred technical solution of the present invention, the specific formation process of the second splicing assembly includes: using the insulating material to bond the side surfaces of the second sub-core to each other to obtain a second splicing assembly, which is used to prepare the inner ring magnetic core after a second heating.
[0065] Preferably, the specific forming process of the third splicing assembly includes: using the insulating material to bond the side surfaces of the third sub-magnetic core to each other to obtain a third splicing assembly, and after a third heating, using it to prepare the outer ring magnetic core.
[0066] Preferably, the temperatures of the second heating and the third heating are each independently 100-180°C, for example, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C, etc.
[0067] Preferably, the second heating and third heating times are each independently 60 to 180 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0068] Preferably, the side surfaces and bottom surfaces of the second sub-magnetic core and the third sub-magnetic core need to be ground before bonding with the insulating material.
[0069] Preferably, the specific preparation process of the inner ring magnetic core and the outer ring magnetic core includes: using the insulating material to respectively stick the bottom surface of the second splicing component after the second heating and the third splicing component after the third heating to the surface of the chassis magnetic core, after the fourth heating, a blank is obtained, and the blank is post-processed to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core to prepare the wireless charging magnetic core.
[0070] Preferably, the second splicing component is adhered to the middle area of the chassis magnetic core.
[0071] Preferably, the third splicing component is adhered to the edge area of the chassis magnetic core.
[0072] Preferably, the temperature of the fourth heating is 100-180°C, for example, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C, etc.
[0073] In the present invention, if the fourth heating temperature is too high, the obtained blank will be easily cracked; if the fourth heating temperature is too low, the adhesive force of the glue is insufficient, causing the second splicing component or the third splicing component to fall off.
[0074] Preferably, the fourth heating time is 60 to 180 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0075] The present invention combines the bonding process and the heating process of the insulating material, which is beneficial to fully solidify the insulating material between the sub-magnetic cores in the blank, realizes effective splicing between the wireless charging magnetic cores, and ensures that the magnetic cores have sufficient strength during CNC processing, grinding, and transportation.
[0076] Preferably, the post-processing includes CNC machining and surface grinding.
[0077] The present invention further performs numerical control processing and surface grinding processing on the formed blank to obtain a wireless charging magnetic core with a desired structure and processing accuracy.
[0078] Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core.
[0079] As a further preferred technical solution of the present invention, the preparation method comprises:
[0080] (1) grinding the side of the first sub-core, and then bonding the side of the first sub-core to each other using an insulating material to form a first splicing assembly, heating the first splicing assembly at 100 to 180° C. for 60 to 180 minutes, and grinding and cutting the heated material to obtain the chassis core;
[0081] (2) grinding the side surfaces and bottom surfaces of the second sub-core and the third sub-core, bonding the side surfaces of the second sub-core to each other using an insulating material, obtaining a second splicing assembly, and using the second splicing assembly for preparing an inner ring magnetic core after a second heating at a temperature of 100 to 180° C. for 60 to 180 min;
[0082] The side surfaces of the third sub-magnetic core are spliced together by using an insulating material to obtain a third spliced assembly, which is used to prepare an outer ring magnetic core after a third heating at a temperature of 100 to 180° C. for 60 to 180 minutes;
[0083] (3) pasting the bottom surfaces of the second splicing component after the second heating and the third splicing component after the third heating to the surface of the chassis magnetic core respectively through insulating materials, wherein the second splicing component is pasted to the middle area of the chassis magnetic core, and the third splicing component is pasted to the edge area of the chassis magnetic core, and then, performing a fourth heating at 100 to 180° C. for 60 to 180 min to obtain a green body;
[0084] (4) Post-processing the blank by CNC machining and surface grinding to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, wherein the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core, thereby preparing the wireless charging magnetic core.
[0085] As another preferred technical solution of the present invention, the specific preparation process of the inner ring magnetic core and the outer ring magnetic core includes:
[0086] The insulating material is used to directly bond the bottom surfaces of the second sub-core and the third sub-core to the surface of the chassis core to form the second splicing assembly and the third splicing assembly respectively. Then, the blank is obtained by heating, and the blank is post-processed to form an inner ring core and an outer ring core on the surface of the chassis core to prepare the wireless charging core.
[0087] The present invention provides a bonding and curing process for the sub-magnetic core directly on the surface of the obtained chassis magnetic core to realize the preparation of the wireless charging magnetic core. Only two heating operations are required in the whole process to prepare the wireless charging magnetic core with a large cross-sectional area and high charging power. The process is simpler and the energy consumption is lower.
[0088] Preferably, the bottom surface of the second sub-magnetic core needs to be ground before being coated with the insulating material.
[0089] Preferably, the bottom surface of the third sub-magnetic core needs to be ground before being coated with the insulating material.
[0090] Preferably, the second splicing component is located in the middle area of the chassis magnetic core.
[0091] Preferably, the third splicing component is located at an edge area of the chassis magnetic core.
[0092] Preferably, the heating temperature is 100-180° C., for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0093] Preferably, the heating time is 60 to 180 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0094] Preferably, the post-processing includes CNC machining and surface grinding.
[0095] Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core.
[0096] As another further preferred technical solution of the present invention, the preparation method comprises:
[0097] (I) grinding the side of the first sub-core, then bonding the side of the first sub-core to each other using an insulating material to form a first splicing assembly, heating the first splicing assembly at 100 to 180° C. for 60 to 180 minutes, grinding and cutting the heated material to obtain the chassis core;
[0098] (II) grinding the bottom surfaces of the second sub-core and the third sub-core, and respectively bonding the bottom surfaces of the second sub-core and the third sub-core to the surface of the chassis core using an insulating material, wherein the second sub-core is bonded to the middle area of the chassis core to form a second splicing assembly in the middle area on the surface of the chassis core, and the third sub-core is bonded to the edge area of the chassis core to form a third splicing assembly in the edge area on the surface of the chassis core, and then heating at a temperature of 100 to 180° C. for 60 to 180 min to obtain a blank;
[0099] (III) Post-processing the blank by CNC machining and surface grinding to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, wherein the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core, thereby preparing the wireless charging magnetic core.
[0100] As a further preferred technical solution of the present invention, the specific process of CNC machining and surface grinding of the blank includes:
[0101] (A) fixing the obtained green body on a workbench of a processing equipment, compiling a CNC processing program according to the design requirements and dimensional accuracy of the magnetic core, using a CNC machine tool to perform rough processing, removing excess material, and then performing fine processing to obtain a magnetic core of the required size and shape;
[0102] (B) The magnetic core obtained in step (A) is ground using a surface grinder to remove processing marks and obtain a final wireless charging magnetic core.
[0103] In the present invention, the spacing area in the outer ring magnetic core or the inner ring magnetic core can be obtained by performing numerical control machining and surface grinding on the blank.
[0104] In a third aspect, the present invention provides an application of the wireless charging magnetic core as described in the first aspect, wherein the wireless charging magnetic core is applied to unmanned warehousing systems, electric vehicle wireless charging systems, intelligent driving or industrial robots.
[0105] The wireless charging magnetic core of the present invention can be used in the fields of high-power electric vehicle wireless charging systems, intelligent driving, unmanned storage systems and industrial robots to achieve automatic charging capabilities.
[0106] Compared with the prior art, the present invention has at least the following beneficial effects:
[0107] (1) The wireless charging magnetic core of the present invention has a large cross-sectional area and can carry a very large charging power;
[0108] (2) The present invention realizes the splicing of sub-cores in the wireless charging magnetic core through insulating materials, and can separate each sub-core through an insulating layer, thereby effectively reducing the eddy current loss of the wireless charging magnetic core and improving the heat dissipation uniformity during operation;
[0109] (3) The present invention adopts CNC machining and surface grinding processes to process the spliced magnetic cores, which has high dimensional accuracy, good product consistency, and can be stably produced in batches. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] Figure 1 It is a top view schematic diagram of the first splicing assembly in Example 1.
[0111] Figure 2 Schematic diagram of a top view of the chassis core in Example 1.
[0112] Figure 3 Schematic diagram of the structure of the wireless charging magnetic core in Example 1.
[0113] Figure 4 It is a top view schematic diagram of the first splicing assembly in Example 2.
[0114] Figure 5 It is a top view schematic diagram of the chassis core in Example 2.
[0115] Figure 6 It is a top view schematic diagram of the position distribution of the second splicing component and the third splicing component of Example 2 on the surface of the chassis core.
[0116] Figure 7 It is a schematic diagram of the structure of the wireless charging magnetic core of Example 2.
[0117] Among them, 1-chassis core, 2-inner ring core, 21-spaced area in the inner ring core, 3-outer ring core, 31-spaced area in the outer ring core, 4-second splicing assembly, 5-third splicing assembly, a1-first side length of the L-shaped cross section of the sub-core, a2-first side width of the L-shaped cross section of the sub-core, b1-second side length of the L-shaped cross section of the sub-core, b2-second side width of the L-shaped cross section of the sub-core. DETAILED DESCRIPTION
[0118] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0119] The first sub-core, the second sub-core and the third sub-core used in the following embodiments are all sub-cores whose side surfaces are perpendicular to the upper and lower bottom surfaces.
[0120] The sub-cores used for splicing in the following embodiments are commercially available, wherein the sub-cores used in the outer ring core, the inner ring core and the chassis core are all made of DMR95 manganese-zinc power ferrite cores.
[0121] The specific process of CNC machining and surface grinding of the obtained green body involved in the following embodiments includes:
[0122] (A) fixing the obtained green body on a workbench of a processing equipment, compiling a CNC processing program according to the design requirements and dimensional accuracy of the magnetic core, using a CNC machine tool to perform rough processing, removing excess material, and then performing fine processing to obtain a magnetic core of the required size and shape;
[0123] (B) The magnetic core obtained in step (A) is ground using a surface grinder to remove processing marks and obtain a final wireless charging magnetic core.
[0124] Example 1
[0125] This embodiment provides a schematic diagram of the structure of a wireless charging magnetic core of model P575. Figure 3 As shown in the figure, it can be seen that the wireless charging magnetic core includes a chassis magnetic core 1 with a circular hole in the center, an inner ring magnetic core 2 located in the middle area on the surface of the chassis magnetic core 1, and the inner ring magnetic core is a concave-convex structure of a circular ring, and an outer ring magnetic core 3 located in the edge area on the surface of the chassis magnetic core 1, and the outer ring magnetic core is also a concave-convex structure of a circular ring, and the outer contour of the outer ring magnetic core 3 is consistent with the outer contour of the chassis magnetic core 1. There are spacing areas 21 and 31 around the inner ring magnetic core 2 and the outer ring magnetic core 3 in the wireless charging magnetic core; the cross-sectional area of the obtained wireless charging magnetic core is 2600cm 2 The chassis core 1, the inner core 2 and the outer core 3 of the wireless charging core are all formed by splicing sub-cores, and there is an insulating layer between each sub-core. The theoretical design rated power of the wireless charging core can reach 60kW.
[0126] This embodiment also provides a method for preparing the wireless charging magnetic core of model P575, the preparation method comprising:
[0127] (1) Grind the side surfaces of 36 first sub-cores with square cross-sections, where the side length of the square is 100 mm and the height of the first sub-core is 8 mm. Then, epoxy resin is used to bond the side surfaces of the first sub-cores to each other to form a first splicing assembly, as shown in a top view. Figure 1 As shown, the length of the first splicing component is 600 mm and the width is 600 mm. The first splicing component is first heated at 120° C. for 90 min to fully cure the epoxy resin. The upper and lower surfaces of the heated material are ground, and according to Figure 1The heated product is cut at the dotted line position in the figure to obtain a chassis core with a circular cross section and a circular diameter of 577.5 mm. The top view thereof is shown in FIG. Figure 2 As shown;
[0128] (2) grinding the side surfaces and bottom surfaces of the four second sub-cores and the eighteen third sub-cores, wherein the cross section of the second sub-core is an arc with an outer diameter of 260 mm, an inner diameter of 180 mm, and an angle of 90°, and the height of the second sub-core is 20 mm; the cross section of the third sub-core is an arc with an outer diameter of 580 mm, an inner diameter of 550 mm, and an angle of 20°, and the height of the third sub-core is 20 mm;
[0129] The side surfaces of the second sub-core are bonded to each other using epoxy resin to obtain a second splicing assembly of a circular ring structure, which is then subjected to a second heating at 120°C for 90 minutes and used to prepare an inner ring magnetic core; the side surfaces of the third sub-core are spliced to each other using epoxy resin to obtain a third splicing assembly of a circular ring structure, which is then subjected to a third heating at 120°C for 90 minutes and used to prepare an outer ring magnetic core.
[0130] (3) using epoxy resin to adhere the bottom surfaces of the second splicing component after the second heating and the third splicing component after the third heating to corresponding positions on the surface of the chassis magnetic core, respectively, wherein the second splicing component is adhered to the middle area of the chassis magnetic core, and the third splicing component is adhered to the edge area of the chassis magnetic core, and then the bonded product is subjected to a fourth heating at 120° C. for 90 minutes to obtain a blank;
[0131] (4) The blank is subjected to CNC machining and surface grinding to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, wherein the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core, the outer ring magnetic core and the inner ring magnetic core both include a spacing area, and the center of the chassis magnetic core has a circular hole, thereby obtaining the wireless charging magnetic core, whose structural schematic diagram is shown in FIG. Figure 3 shown.
[0132] Example 2
[0133] This embodiment provides a wireless charging magnetic core of model P355, and its structural diagram is as follows: Figure 7 As shown in the figure, it can be seen that the wireless charging magnetic core includes a chassis magnetic core 1 with a circular hole in the center, an inner ring magnetic core 2 located in the middle area on the surface of the chassis magnetic core 1, and the inner ring magnetic core 2 is a square ring structure closed on all sides, and an outer ring magnetic core 3 located in the edge area on the surface of the chassis magnetic core 1, and the outer ring magnetic core 3 is a square ring structure with spacing areas 31 on all sides, and the outer contour of the outer ring magnetic core 3 is consistent with the outer contour of the chassis magnetic core 1; the cross-sectional area of the obtained wireless charging magnetic core is 1280cm 2Moreover, the chassis core 1, the inner core 2 and the outer core 3 of the wireless charging core are all formed by splicing sub-cores, and there is an insulating layer between each sub-core. The theoretical design rated power of the wireless charging core can reach 35kw.
[0134] This embodiment also provides a method for preparing the wireless charging magnetic core of the model P355, the preparation method comprising:
[0135] (1) Grind the side surfaces of 16 first sub-cores with square cross-sections, where the side length of the square is 90 mm and the height of the first sub-core is 10 mm. Then, epoxy resin is used to bond the side surfaces of the first sub-cores to each other to form a first splicing assembly, as shown in a top view. Figure 4 As shown, the cross-section length of the first splicing component is 360 mm and the width is 360 mm. The first splicing component is first heated at 120° C. The first heating time is 120 min to fully cure the epoxy resin. The upper and lower surfaces of the heated material are ground, and according to Figure 4 The heated product is cut at the dotted line position in the figure. The shape of the cross section after cutting is as follows: Figure 5 As shown, the chassis magnetic core is obtained;
[0136] (2) The side surfaces and bottom surfaces of four second sub-cores with L-shaped cross sections are ground. The length a1 of the first side of the L-shaped cross section of the second sub-core is 120 mm, the width a2 of the first side is 40 mm, the length b1 of the second side is 120 mm, the width b2 of the second side is 40 mm, the first side and the second side of the L-shaped cross section are transitioned by rounded corners, the height of the second sub-core is 22.5 mm, and its specific shape is as follows: Figure 6 As shown; the side and bottom surfaces of the third sub-core are ground. The third sub-core is composed of 4 sub-cores with arc-shaped cross sections and 12 sub-cores with rectangular cross sections, wherein the arc has an outer diameter of 150 mm, an inner diameter of 130 mm, and an angle of 90°. The length and width of the rectangle are 70 mm and 10 mm, and the height of the second sub-core is 22.5 mm.
[0137] The side surfaces of the second sub-core are bonded to each other using epoxy resin to obtain a second splicing assembly of a square ring structure, which is then subjected to a second heating at 120°C for 90 minutes to prepare an inner ring magnetic core; the side surfaces of the third sub-core are spliced to each other using epoxy resin, which is then subjected to a third heating at 120°C for 90 minutes to obtain a third splicing assembly of a square ring structure to prepare an outer ring magnetic core.
[0138] (3) using epoxy resin to adhere the bottom surfaces of the second splicing component after the second heating and the third splicing component after the third heating to corresponding positions on the surface of the chassis magnetic core, respectively, the second splicing component is adhered to the middle area of the chassis magnetic core, and the third splicing component is adhered to the edge area of the chassis magnetic core, and then the bonded product is subjected to a fourth heating at 120° C. for 150 min to obtain a blank;
[0139] (4) The blank is subjected to CNC machining and surface grinding to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, wherein the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core, the outer ring magnetic core includes a spacing area, and the inner ring magnetic core does not include a spacing area, and the center of the chassis magnetic core has a circular hole, thereby obtaining the wireless charging magnetic core, whose structural schematic diagram is shown in FIG. Figure 7 shown.
[0140] The top view schematic diagram of the distribution of the first splicing component and the second splicing component on the surface of the chassis magnetic core in the preparation method provided in this embodiment is as follows Figure 6 As shown in the figure, it can be seen that the second splicing component 4 is located in the middle area of the chassis core 1, corresponding to the square ring structure composed of four second sub-cores with L-shaped cross-sections, and the third splicing component 6 is located in the edge area of the chassis core 1, and its outer contour is consistent with the outer contour of the chassis core 1, corresponding to the square ring structure composed of 4 third sub-cores with arc-shaped cross-sections and 12 third sub-cores with rectangular cross-sections.
[0141] Example 3
[0142] This embodiment provides a method for preparing a wireless charging magnetic core, which differs from the first embodiment only in that the epoxy resin used in the preparation method is replaced with AB glue, the first heating, the second heating, the third heating and the fourth heating are all at 100°C, and the heat preservation time is 180 minutes. The rest is the same as the first embodiment.
[0143] Example 4
[0144] This embodiment provides a method for preparing a wireless charging magnetic core, which is different from the first embodiment in that the first, second, third and fourth heating temperatures in the preparation method are all 180° C., and the heat preservation time is all 60 minutes. The rest is the same as the first embodiment.
[0145] Example 5
[0146] The wireless charging magnetic core of model P575 provided in this embodiment is the same as that provided in embodiment 1. The difference between this embodiment and embodiment 1 is that the preparation method of the wireless charging magnetic core provided in this embodiment includes the following steps:
[0147] (I) Grinding the side surfaces of 36 first sub-cores with square cross-sections, where the side length of the square is 100 mm and the height of the first sub-core is 8 mm, then bonding the side surfaces of the first sub-cores to each other with epoxy resin to form a first splicing assembly, the top view of which is shown in FIG. Figure 1 As shown, the length of the first splicing component is 600 mm and the width is 600 mm. The first heating is performed at 120° C. for 90 min to fully cure the epoxy resin. The upper and lower surfaces of the heated material are ground, and according to Figure 1 The heated product is cut at the dotted line position in the figure to obtain a chassis core with a circular cross section and a circular diameter of 577.5 mm. The top view schematic diagram is shown in FIG. Figure 2 As shown;
[0148] (II) grinding the bottom surfaces of 4 second sub-cores and 18 third sub-cores, wherein the second sub-core has an outer diameter of 260 mm, an inner diameter of 180 mm, and an arc angle of 90°, and the height of the second sub-core is 20 mm; the third sub-core has an outer diameter of 580 mm, an inner diameter of 550 mm, and an arc angle of 20°, and the height of the third sub-core is 20 mm;
[0149] Adhere the bottom surfaces of the second sub-core and the third sub-core to the surface of the chassis core respectively by using epoxy resin, wherein the second sub-core is adhered to the middle area of the chassis core to form a second splicing assembly in the middle area on the surface of the chassis core, and the third sub-core is adhered to the edge area of the chassis core to form a third splicing assembly in the edge area on the surface of the chassis core, and then heat the bonded product at 120° C. for 90 minutes to obtain a green body;
[0150] (III) Post-processing the blank by CNC machining and surface grinding to form an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, wherein the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core, and both the outer ring magnetic core and the inner ring magnetic core include a spacing area, and the center of the chassis magnetic core has a circular hole, so as to prepare the wireless charging magnetic core, whose structural schematic diagram is shown in FIG. Figure 3 shown.
[0151] In summary, the present invention realizes the splicing of the sub-cores in the wireless charging magnetic core by using insulating materials, and realizes the precise positioning of the sub-cores by numerical control processing and high-precision grinding of the spliced blank. The large-scale wireless charging magnetic core prepared by the present invention can effectively reduce the eddy current loss of the wireless charging magnetic core and improve its heat dissipation uniformity during operation because the sub-cores are separated by insulating materials.
[0152] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A wireless charging magnetic core, characterized in that: The wireless charging magnetic core comprises a chassis magnetic core, an inner ring magnetic core and an outer ring magnetic core located on the surface of the chassis magnetic core, and the cross-sectional area of the wireless charging magnetic core is 500cm 2 In the above, the chassis magnetic core, the inner ring magnetic core and the outer ring magnetic core each include at least two sub-magnetic cores and an insulating layer located between the sub-magnetic cores.
2. The wireless charging magnetic core according to claim 1, characterized in that: The inner ring magnetic core is located in the middle area on the surface of the chassis magnetic core; Preferably, there is a spacing area in the inner ring magnetic core; Preferably, the outer ring magnetic core is located in the edge area on the surface of the chassis magnetic core; Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core; Preferably, there is a spacing area in the outer ring magnetic core; Preferably, the charging power of the wireless charging magnetic core is 20-60kW; Preferably, the structure of the inner ring magnetic core includes any one of a square ring, a circular ring, a racetrack type or a concave-convex structure, or a combination of at least two thereof; Preferably, the structure of the outer ring magnetic core includes any one of a square ring, a circular ring or a concave-convex structure, or a combination of at least two of them.
3. A method for preparing a wireless charging magnetic core according to claim 1 or 2, characterized in that: The preparation method comprises: The sub-magnetic cores are spliced into a chassis magnetic core and an inner ring magnetic core and an outer ring magnetic core located on the surface of the chassis magnetic core through insulating materials to obtain the wireless charging magnetic core.
4. The preparation method according to claim 3, characterized in that: The cross-section of the sub-magnetic core includes any one of square, rectangle, arc, ring, trapezoid, L-shape or concave-convex shape or a combination of at least two thereof; Preferably, the side length of the square is 50 to 120 mm; Preferably, the length of the rectangle is 50 to 150 mm; Preferably, the width of the rectangle is 5 to 120 mm; Preferably, the included angle of the arc is 0 to 180° and does not include 0°; Preferably, the outer diameter of the arc or ring is independently selected from 150 to 600 mm; Preferably, the inner diameter of the arc or ring is independently selected from 50 to 550 mm; Preferably, the length of the first side of the L-shape is 50 to 150 mm; Preferably, the width of the first side of the L-shape is 20 to 50 mm; Preferably, the length of the second side of the L-shape is 50 to 150 mm; Preferably, the width of the second side of the L-shape is 20-50 mm.
5. The preparation method according to claim 3 or 4, characterized in that: The sub-magnetic core comprises a first sub-magnetic core, a second sub-magnetic core and a third sub-magnetic core; Preferably, the first sub-cores are spliced to form a first spliced assembly for preparing a chassis magnetic core; Preferably, the second sub-cores are spliced to form a second splicing assembly for preparing an inner ring magnetic core; Preferably, the third sub-magnetic cores are spliced to form a third splicing assembly, which is used to prepare an outer ring magnetic core; Preferably, the first sub-core, the second sub-core and the third sub-core all comprise a manganese-zinc power ferrite core; Preferably, the insulating material includes insulating glue; Preferably, the insulating glue includes any one of epoxy resin, AB glue or polyurethane glue.
6. The preparation method according to claim 5, characterized in that: The specific preparation process of the chassis magnetic core includes: using the insulating material to bond the side surfaces of the first sub-magnetic core to each other to form a first splicing assembly, and after a first heating, obtaining the chassis magnetic core; Preferably, the side surface of the first sub-magnetic core needs to be ground before coating the insulating material; Preferably, the first heating temperature is 100-180°C; Preferably, the first heating time is 60 to 180 minutes; Preferably, before preparing the chassis magnetic core, the first heated material is further subjected to grinding and cutting processing.
7. The preparation method according to claim 5 or 6, characterized in that: The specific forming process of the second splicing assembly includes: using the insulating material to bond the side surfaces of the second sub-magnetic core to each other to obtain a second splicing assembly, and after a second heating, using it to prepare the inner ring magnetic core; Preferably, the specific forming process of the third splicing assembly includes: using the insulating material to bond the side surfaces of the third sub-magnetic core to each other to obtain a third splicing assembly, and after a third heating, using the third splicing assembly to prepare the outer ring magnetic core; Preferably, the second heating and the third heating temperatures are independently 100 to 180°C; Preferably, the second heating and the third heating time are each independently 60 to 180 minutes; Preferably, the side surfaces and bottom surfaces of the second sub-magnetic core and the third sub-magnetic core need to be ground before bonding with the insulating material.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The specific preparation process of the inner ring magnetic core and the outer ring magnetic core includes: using the insulating material to respectively adhere the bottom surfaces of the second splicing component after the second heating and the third splicing component after the third heating to the surface of the chassis magnetic core, after the fourth heating, to obtain a blank, post-processing the blank, forming an inner ring magnetic core and an outer ring magnetic core on the surface of the chassis magnetic core, and preparing the wireless charging magnetic core; Preferably, the second splicing component is adhered to the middle area of the chassis magnetic core; Preferably, the third splicing component is adhered to the edge area of the chassis magnetic core; Preferably, the temperature of the fourth heating is 100-180°C; Preferably, the fourth heating time is 60 to 180 minutes; Preferably, the post-processing includes CNC machining and surface grinding; Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core.
9. The preparation method according to claim 5 or 6, characterized in that: The specific preparation process of the inner ring magnetic core and the outer ring magnetic core includes: The insulating material is used to directly bond the bottom surfaces of the second sub-core and the third sub-core to the surface of the chassis core, respectively, to form the second splicing assembly and the third splicing assembly, respectively; then, after heating, a blank is obtained, and the blank is post-processed to form an inner ring core and an outer ring core on the surface of the chassis core, thereby preparing the wireless charging core. Preferably, the bottom surface of the second sub-magnetic core needs to be ground before being coated with the insulating material; Preferably, the bottom surface of the third sub-magnetic core needs to be ground before being coated with the insulating material; Preferably, the second splicing component is located in the middle area of the chassis magnetic core; Preferably, the third splicing component is located at the edge area of the chassis magnetic core; Preferably, the heating temperature is 100-180°C; Preferably, the heating time is 60 to 180 minutes; Preferably, the post-processing includes CNC machining and surface grinding; Preferably, the outer contour of the outer ring magnetic core is consistent with the outer contour of the chassis magnetic core.