Lead frame silver coating removing and bonding method

Through laser ablation and deoxidation treatment technology, the problem of strong customization properties, high cost and long cycle of the lead frame silver plating layer removal method is solved, and the transformation of ordinary silver plating frames to point-area silver plating frames is realized, improving the Reliability of plastic sealing devices.

CN118969629APending Publication Date: 2024-11-15ZHENGZHOU XINGHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034020.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the silver plating layer removal method of lead frame has problems such as strong customization properties, high cost and long cycle, and it is difficult to achieve the conversion of an ordinary silver plating frame to a point-area silver plating frame.

Method used

By determining the bonding area of ​​the silver plating layer that needs to be retained based on the bonding diagram, laser ablation is used to remove other silver plating areas, and deoxidize the lead frame for partial silver plating layer removal, realizing the preparation of customized silver plating areas .

Benefits of technology

It realizes the rapid transformation of ordinary silver-plated frames into point-area silver-plated frames, reducing costs and cycles, and improving the reliability of plastic packaging devices. It is suitable for customized packaging of high-reliability plastic packaging devices in small batches and various types.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004970604760000011
    Figure HDA0004970604760000011
  • Figure HDA0004970604760000012
    Figure HDA0004970604760000012
  • Figure HDA0004970604760000021
    Figure HDA0004970604760000021
Patent Text Reader

Abstract

The invention provides a lead frame silver plating layer removing and bonding method, and the method comprises the steps: S1, determining a silver plating layer bonding region which needs to be reserved on the surface of a lead frame according to a bonding graph; s2, performing laser ablation on a silver-plated area except the silver-plated layer bonding area on the surface of the lead frame; and S3, carrying out deoxidation treatment on the lead frame obtained in the S2, and then cleaning the lead frame. The reserved silver plating layer bonding area is determined according to the bonding area required for packaging the bonding graph, other silver plating areas except the reserved silver plating layer bonding area are ablated through a laser ablation method, unnecessary silver plating areas are removed, preparation of the lead frame with the customized silver plating area is achieved, and the production efficiency of the lead frame with the customized silver plating area is improved. And the effect of silver-plated frame in a point area is achieved. According to the method, the problems of high customization attribute, high cost, long period and the like of a traditional point area silver-plated frame are solved while a common carrier full silver-plated and ring silver-plated lead frame is quickly and simply changed into the point area silver-plated frame.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor integrated circuit packaging and testing, and relates to a lead frame silver plating layer removal and bonding method. Background Art

[0002] The lead frame substrate used in semiconductor packaging is copper, but copper is easily oxidized and is not conducive to packaging bonding. Therefore, a silver-plated layer is usually plated in specific areas. The silver-plated layer is mainly used as a bonding area to achieve the interconnection between the chip bonding pad and the lead frame silver-plated bonding area, and complete the electrical connection between the chip and the lead frame. In the lead frame production process, silver plating requires a special silver-plated mask mold. In order to achieve the versatility of the lead frame to cope with various bonding patterns, the silver-plated mask mold has a large window, resulting in a relatively large silver-plated area. Common regional modes include full carrier silver plating, double ring silver plating, and single ring silver plating. In addition, there is point area silver plating, that is, silver plating is performed in the area where bonding is required, and the silver-plated area is slightly larger than the area required for bonding. Point area silver plating requires a special silver-plated mask mold, which is not very versatile. During the packaging process, different bonding patterns have different requirements for the silver-plated area. There is usually a problem of too large a silver-plated area, that is, the bonding area of ​​the silver-plated layer is significantly smaller than the area of ​​the silver-plated layer.

[0003] The area of ​​the silver-plated layer is too large, which is not conducive to the reliability of semiconductor package plastic sealed devices, mainly because the bonding strength between the plastic powder and the silver-plated layer is about 50% of the bonding strength between the plastic powder and the copper substrate of the lead frame. For the lead frame with a fully silver-plated carrier, the surface of the frame carrier is completely silver-plated, and the tip of the lead in the frame is silver-plated. The area of ​​the silver-plated area occupies more than 40% of the total area of ​​the frame inside the plastic package, which has an adverse effect on the reliability of the plastic sealed device. In the high-reliability plastic sealing fields such as military and automobiles, in order to minimize the area of ​​the silver-plated area to improve the overall reliability of the plastic sealed device, customized point area silver plating design is usually performed.

[0004] The specific technology for making the point area silver-plated frame is as follows: (1) determining the position of the area of ​​the lead frame that needs to be silver-plated based on the bonding diagram, and designing the drawings for the point areas that need to be silver-plated; (2) making a silver-plating mask mold based on the design drawings for the point area silver-plating; (3) in the silver-plating process, using a customized point area silver-plating mask mold to cover the surface of the lead frame substrate, covering the area that is not silver-plated and exposing the area that needs to be silver-plated; (4) completing the production of the point area silver-plated frame according to the lead frame processing flow.

[0005] Currently, the industry lacks an effective method to remove the silver plating layer of the lead frame. The only way is to make a lead frame with a specific silver plating pattern according to the needs when making the lead frame. The main problems with the point area silver plating method are: (1) the customization property is too strong, and it is impossible to transform the ordinary silver-plated frame into the point area silver-plated frame; (2) the cost is high, and a specific silver plating mask mold needs to be prepared in advance; (3) the cycle is long, and the point area silver plating design and the production and processing of the specific silver plating mask mold increase the processing cycle of the frame. Summary of the invention

[0006] The purpose of the present invention is to provide a method for removing the silver-plated layer of a lead frame and bonding it, so as to solve the problems of strong customization properties, high cost and long cycle of the silver-plated frame in the midpoint area of ​​the prior art.

[0007] The present invention is achieved through the following technical solutions:

[0008] A method for removing a silver-plated layer of a lead frame, comprising:

[0009] S1, according to the bonding diagram, determine the silver-plated bonding area on the lead frame surface that needs to be retained;

[0010] S2, laser ablation of the silver-plated area on the surface of the lead frame except for the silver-plated layer bonding area;

[0011] S3, deoxidizing the lead frame obtained in S2, and then cleaning it.

[0012] Preferably, in S1, the silver-plated layer bonding area is set as a rectangle or a square, with a width of more than 2 times and less than 5 times the size of the frame bonding point in the same direction, and a length of more than 2 times and less than 5 times the size of the frame bonding point in the same direction.

[0013] Preferably, in S2, the laser used for laser ablation is an ultraviolet laser.

[0014] Furthermore, in S2, the wavelength of the ultraviolet laser is 355 nm.

[0015] Preferably, in S2, the power used for laser ablation is 20W-40W.

[0016] Preferably, in S2, the laser ablation rate is 600 mm / s to 1200 mm / s.

[0017] Preferably, in S3, the deoxidation treatment of the lead frame obtained in S2 is specifically: immersing the lead frame obtained in S2 in a deoxidation solution.

[0018] Furthermore, the deoxidation solution is 80 g / L to 120 g / L sodium persulfate solution, and the soaking temperature is 30° C. to 40° C.

[0019] Preferably, the method further comprises: S4, placing the lead frame obtained in S3 in a protective aqueous solution at room temperature for anti-discoloration treatment to obtain a lead frame with a partially removed silver plating layer.

[0020] The present invention provides a lead frame bonding method, comprising: bonding a chip to a lead frame obtained by the lead frame silver-plated layer removal method as described above, curing and baking, bonding one end of a bonding wire to a chip pad, and then bonding the other end of the bonding wire to the center position of a silver-plated layer bonding area on the lead frame.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention determines the reserved silver-plated layer bonding area according to the bonding area required by the package bonding diagram, and ablates other silver-plated areas outside the reserved silver-plated layer bonding area by laser ablation, removes unnecessary silver-plated areas, realizes the preparation of customized silver-plated area lead frame, and achieves the effect of point area silver-plated frame. The method of the present invention can quickly and easily realize the transformation of ordinary carrier full silver-plated and ring silver-plated lead frame into point area silver-plated frame, while reducing the problems of strong customized properties, high cost, long cycle, etc. of traditional point area silver-plated frame. The lead frame formed by the present invention has a bonding area that matches the position of the silver-plated area. When bonding, the bonding point is just in the reserved silver-plated layer bonding area, which reduces the total area of ​​the silver-plated area, improves the bonding force between the plastic powder inside the plastic-sealed device and the frame, and improves the reliability of the plastic-sealed device. It is suitable for customized packaging of small batches and multiple types of high-reliability plastic-sealed devices. While removing the silver-plated layer by laser ablation, the present invention generates an oxidation reaction on the copper base layer in the burnt area. The oxidized copper layer will reduce its bonding strength with the plastic powder and affect the reliability of the device. The present invention removes the copper oxide generated by laser ablation through deoxidation treatment, thereby avoiding the influence of copper oxide on the bonding strength.

[0023] Furthermore, considering the reflective characteristics of the silver-plated layer, the present invention selects ultraviolet laser to perform laser ablation of the silver-plated layer of the lead frame, which can improve the ablation effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a schematic diagram of the front view of a common lead frame.

[0026] Figure 2Schematic diagram of ordinary lead frame bonding.

[0027] Figure 3 Schematic diagram of laser ablation of non-retained silver-plated areas of the lead frame.

[0028] Figure 4 Schematic diagram of the laser ablation effect on the silver-plated area.

[0029] Figure 5 Schematic diagram of lead frame bonding after ablation.

[0030] In the figure: 1-lead frame carrier silver-plated area, 2-lead frame pin silver-plated area, 3-lead frame copper substrate, 4-chip, 5-chip pad, 6-bonding wire, 7-two solder joints, 8-lead frame carrier silver-plated ablation area, 9-lead frame inner pin silver-plated ablation area, 10-lead frame copper substrate. DETAILED DESCRIPTION

[0031] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0032] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0033] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0034] The method for removing the silver-plated layer of the lead frame and bonding thereof of the present invention performs secondary processing on the full silver-plated and ring silver-plated frames of the ordinary carrier before the packaging process to reduce the surface silver-plated area and meet the silver-plated layer bonding area. According to the bonding diagram, the silver-plated layer bonding area to be retained and the silver-plated area to be removed are determined, and the silver-plated area to be removed is ablated by laser equipment, and then chemical deoxidation and organic protective layer anti-discoloration treatment are used to complete the transformation of the ordinary silver-plated frame into a point area silver-plated frame. Afterwards, the treated point area silver-plated frame is used for fixed point area bonding.

[0035] The specific implementation process of the present invention includes the following steps:

[0036] (1) Selection and positioning method of the silver-plated bonding area that needs to be retained and the silver-plated area that needs to be removed on the lead frame

[0037] Figure 1 This is a front view of a common lead frame, which is a carrier fully silver-plated lead frame, and the frame carrier and the tips of the pins in the frame are silver-plated areas. In addition to the lead frame copper substrate 3, the lead frame carrier silver-plated area 1 and the lead frame pin silver-plated area 2 are all silver-plated areas.

[0038] Figure 2 The schematic diagram of the bonding of a common lead frame is shown in FIG. The chip pad 5 on the chip 4 is used as the chip signal lead-out terminal, and the signal is led out to the silver-plated area 2 of the lead frame through the bonding wire 6. A solder joint is formed at the chip end, and two solder joints 7 are formed in the silver-plated area, and the two solder joints 7 are in a fishtail shape.

[0039] The present invention mainly aims to remove the redundant silver-plated area and realize bonding in the reserved silver-plated area (silver-plated layer bonding area).

[0040] First, on the lead frame surface ( Figure 1 )Preserve the bond graph( Figure 2 ) The silver-plated area (silver-plated layer bonding area) required for bonding. The silver-plated layer bonding area is set in a rectangular or square shape, with a width of more than 2 times and less than 5 times the size of the frame bonding point in the same direction, and a length of more than 2 times and less than 5 times the size of the frame bonding point in the same direction. Figure 3 Other silver-plated areas outside the silver-plated layer bonding area need to be removed by laser ablation, including the lead frame carrier silver-plated ablation area 8 and the lead frame inner pin silver-plated ablation area 9.

[0041] Secondly, visual reference points need to be made to enable the laser equipment to automatically locate the silver-plated area that needs to be removed on the lead frame of each device. The visual recognition system of the laser equipment is used to make more than two visual reference points on the front of the lead frame for each device. The visual reference points need to have a unique pattern and can be set in various forms such as diagonal or triangular.

[0042] (2) Selection of light source, power, and rate for laser ablation of the silver-plated layer of the lead frame

[0043] The silver-plated layer has good reflective properties for lasers, and its reflective effect on lasers with a wavelength of 600nm-1000nm is most obvious. Its reflective ability for ultraviolet light is weaker than that of infrared light (wavelength 1064nm) and green light (wavelength 532nm). Therefore, considering the reflective properties of the silver-plated layer, the present invention selects ultraviolet laser to perform laser ablation of the silver-plated layer of the lead frame, and the wavelength of the ultraviolet laser is 355nm. In terms of power, the silver-plated layer can be removed, and the thickness of the silver-plated layer is less than 1μm. The ultraviolet laser power is selected from 20w to 40w. In terms of ablation rate, considering the consistency of ablation, the ablation rate is reduced as much as possible, and the ablation rate is 600mm / s to 1200mm / s. The number of ablations can be 1 time or multiple times.

[0044] (3) Laser ablation of silver-plated layer and deoxidation process

[0045] a. Place the front face of the fully silver-plated or ring-silver-plated lead frame on the workbench of the laser equipment, and ablate the silver-plated area to be removed on the surface according to the above step (1) to form a Figure 4 The laser ablation area shown is the lead frame copper substrate 10 exposed after ablation. After laser ablation, the surface of the lead frame silver plating layer becomes rough, and the height difference of the surface after ablation is 1-3 μm, thereby achieving the removal of the silver plating layer.

[0046] b. Place the lead frame that has been laser ablated as described above in a deoxidation solution for deoxidation treatment, and rinse with pure water after the deoxidation treatment. Considering that the main component of deoxidation is copper oxide, and to prevent the silver plating layer and the copper substrate from being corroded, the deoxidation solution is selected as 80g / L to 120g / L sodium persulfate solution, and the treatment temperature is 30℃ to 40℃.

[0047] c. Place the lead frame that has been deoxidized and rinsed with pure water in a protective aqueous solution at room temperature, and perform anti-discoloration treatment on the lead frame to obtain a lead frame with a partially removed silver plating layer.

[0048] (4) Bonding process of lead frame with partial silver plating removal

[0049] The lead frame with the silver-plated layer partially removed is used for packaging. The chip is bonded, cured and baked, and then the chip pad is interconnected with the silver-plated bonding area of ​​the lead frame. Figure 5 As shown in the figure, after the bonding wire is bonded to the chip pad (solder point 1), it is bonded to the center of the bonding area of ​​the silver-plated layer (solder point 2). A distance larger than the size of the second solder point is reserved around the second solder point (front, back, left, and right) to ensure that the second solder point is bonded to the silver-plated layer that is not affected by laser ablation. The non-reserved silver-plated area becomes the copper substrate exposed and is directly combined with the plastic powder during encapsulation.

[0050] Embodiment 1:

[0051] For a 5-row, 28-column non-roughened SOP8 lead frame, the frame is 228.2952mm long and 50.8mm wide, the carrier is 95mil×130mil, the carrier is fully silver-plated, and there are silver-plated areas on the 8 inner pins. Each inner pin needs to be bonded with one second solder joint. The specific implementation steps are as follows:

[0052] Step 1: Use automatic loading mode or manual mode to place the SOP8 lead frame on the carrier of the laser equipment;

[0053] Step 2: Use the software system of the laser equipment to select a window for the SOP8 lead frame with a matrix window (one window corresponds to one device package) and select the silver-plated area that needs laser ablation. Select all the silver-plated areas on the SOP8 lead frame carrier by ablation, and select the silver-plated areas of inner pin 1, inner pin 2, inner pin 3, inner pin 4, inner pin 5, inner pin 6, inner pin 7, and inner pin 8 except the silver-plated layer bonding area (silver-plated reserved area) that needs to be retained by ablation in a rectangular or square shape;

[0054] Step 3: Use the software system of the laser equipment to set visual reference points on the upper right corner and lower left corner of the front side of the SOP8 lead frame with the selected window;

[0055] Step 4: Copy steps 2 and 3 to other windows on the front of the SOP8 lead frame to select and locate all areas to be laser ablated on the front of the SOP8 lead frame, and save the program;

[0056] Step 5: Use a UV laser light source with a wavelength of 355nm, set the laser ablation power to 20w, the ablation rate to 600mm / s, and the ablation times to 2 times, and complete the laser ablation of the selected silver-plated area of ​​the SOP8 lead frame according to the aforementioned procedure;

[0057] Step 6: Immerse the laser ablated SOP8 lead frame in a sodium persulfate solution with a concentration of 80 g / L, set the temperature to 30°C, and set the time to 1 min;

[0058] Step 7: Rinse the SOP8 lead frame obtained in step 6 with pure water for 30 seconds using flowing pure water;

[0059] Step 8: Immerse the SOP8 lead frame obtained in step 7 in a 30% protective aqueous solution CU-1806 for 30 seconds, and then dry at 70° C. to obtain a SOP8 lead frame with a portion of the silver plating layer removed.

[0060] Step 9: Use the SOP8 lead frame obtained in step 8 to perform chip bonding, and then cure and bake;

[0061] Step 10: Use the aforementioned bonded chip and lead frame combination to bond wires according to the bonding diagram. The two solder joints on the lead frame are bonded to the center of the silver-plated bonding area, thereby achieving interconnection between the chip pad and the silver-plated area of ​​the lead frame.

[0062] Embodiment 2:

[0063] For a 5-row, 28-column non-roughened SOP8 lead frame, the frame is 228.2952mm long and 50.8mm wide, the carrier is 90mil×90mil, the carrier is double-ring silver-plated, 8 inner pins have silver-plated areas, inner pins 2 and 3 are not bonded with two solder joints, and the other inner pins are bonded with one two solder joint each. The specific implementation steps are as follows:

[0064] Step 1: Use automatic loading mode or manual mode to place the SOP8 lead frame on the carrier of the laser equipment;

[0065] Step 2: Use the software system of the laser equipment to select a window for the SOP8 lead frame with a matrix window (one window corresponds to one device package) and select the silver-plated area that needs laser ablation. Select all the silver-plated areas on the SOP8 lead frame carrier for ablation, select all the silver-plated areas on inner pins 2 and 3 for ablation, and select the silver-plated areas of inner pins 1, 4, 5, 6, 7, and 8 except the silver-plated layer bonding area for rectangular or square ablation;

[0066] Step 3: Use the software system of the laser equipment to set visual reference points on the upper right corner and lower left corner of the front side of the SOP8 lead frame with the selected window;

[0067] Step 4: Copy steps 2 and 3 to other windows on the front of the SOP8 lead frame to select and locate all areas to be laser ablated on the front of the SOP8 lead frame, and save the program;

[0068] Step 5: Use a UV laser light source with a wavelength of 355nm, set the laser ablation power to 40w, the ablation rate to 1200mm / s, and the ablation times to 3 times, and complete the laser ablation of the selected silver-plated area of ​​the SOP8 lead frame according to the aforementioned procedure;

[0069] Step 6: Immerse the laser ablated SOP8 lead frame in a sodium persulfate solution with a concentration of 120 g / L, set the temperature to 40°C, and set the time to 50 seconds;

[0070] Step 7: Rinse the SOP8 lead frame obtained in step 6 with pure water for 30 seconds using flowing pure water;

[0071] Step 8: Immerse the SOP8 lead frame obtained in step 7 in a 30% protective aqueous solution CU-1806 for 30 seconds, and then dry at 70° C. to obtain a SOP8 lead frame with a portion of the silver plating layer removed.

[0072] Step 9: Use the SOP8 lead frame obtained in step 8 to perform chip bonding, and then cure and bake;

[0073] Step 10: Use the aforementioned bonded chip and SOP8 lead frame combination, bond the leads according to the bonding diagram, and bond the two solder joints on the SOP8 lead frame to the center of the retained silver-plated layer bonding area, thereby achieving interconnection between the chip pad and the silver-plated area of ​​the SOP8 lead frame.

[0074] Embodiment 3:

[0075] For a 5-row, 6-column non-roughened SOP28 lead frame, the frame is 213.360mm long and 58.420mm wide, the carrier is 150mil×190mil, the carrier is fully silver-plated, 28 inner pins have silver-plated areas, inner pin 14 is bonded to 3 two-solder points, inner pin 20 is not bonded to two-solder points, and other inner pins are bonded to 1 two-solder point each, and there are ground wire bonds around. The specific implementation steps are as follows:

[0076] Step 1: Use automatic loading mode or manual mode to place the SOP28 lead frame on the carrier of the laser equipment;

[0077] Step 2: Use the software system of the laser equipment to select a window for the SOP28 lead frame with a matrix window (one window corresponds to one device package) and select the silver-plated area that needs to be laser ablated. The silver-plated area on the SOP8 lead frame carrier is selected for ablation: (1) The silver-plated area on the inner pin 14 is not selected for ablation, the silver-plated area on the inner pin 20 is selected for ablation, and the silver-plated area of ​​other inner pins except the silver-plated layer bonding area is selected for rectangular or square ablation; (2) The center area of ​​the carrier 130mil×170mil is selected for rectangular ablation.

[0078] Step 3: Use the software system of the laser equipment to set visual reference points on the upper right corner and lower left corner of the front side of the SOP28 lead frame with the selected window;

[0079] Step 4: Copy steps 2 and 3 to other windows on the front of the SOP28 lead frame to select and locate all areas to be laser ablated on the front of the SOP28 lead frame, and save the program;

[0080] Step 5: Use a UV laser light source with a wavelength of 355nm, set the laser ablation power to 30w, the ablation rate to 800mm / s, and the ablation times to 3 times, and complete the laser ablation of the selected silver-plated area of ​​the SOP28 lead frame according to the aforementioned procedure;

[0081] Step 6: Immerse the laser-ablated SOP28 lead frame in a sodium persulfate solution with a concentration of 100 g / L, set the temperature to 35°C, and set the time to 55 seconds;

[0082] Step 7: Rinse the SOP28 lead frame obtained in step 6 with pure water for 30 seconds using running pure water;

[0083] Step 8: Immerse the SOP28 lead frame obtained in step 7 in a 30% protective aqueous solution CU-1806 for 30 seconds, and then dry at 70° C. to obtain a SOP8 lead frame with a portion of the silver plating layer removed.

[0084] Step 9: Use the SOP28 lead frame obtained in step 8 to perform chip bonding, and then cure and bake;

[0085] Step 10: Use the aforementioned bonded chip and SOP28 lead frame combination to bond wires according to the bonding diagram. The two solder joints on the SOP28 lead frame are bonded to the center of the retained silver-plated layer bonding area, thereby achieving interconnection between the chip pad and the silver-plated area of ​​the SOP28 lead frame.

[0086] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for removing a silver-plated layer of a lead frame, characterized in that: include: S1, according to the bonding diagram, determine the silver-plated bonding area on the lead frame surface that needs to be retained; S2, laser ablation of the silver-plated area on the surface of the lead frame except for the silver-plated layer bonding area; S3, deoxidizing the lead frame obtained in S2, and then cleaning it.

2. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: In S1, the silver-plated layer bonding area is set as a rectangle or a square, with a width of more than 2 times and less than 5 times the size of the frame bonding point in the same direction, and a length of more than 2 times and less than 5 times the size of the frame bonding point in the same direction.

3. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: In S2, the laser used for laser ablation is ultraviolet laser.

4. The method for removing the silver plating layer of a lead frame according to claim 3, characterized in that: In S2, the wavelength of the ultraviolet laser is 355 nm.

5. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: In S2, the power used for laser ablation is 20W-40W.

6. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: In S2, the laser ablation rate is 600 mm / s to 1200 mm / s.

7. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: In S3, the deoxidation treatment of the lead frame obtained in S2 is specifically: immersing the lead frame obtained in S2 in a deoxidation solution.

8. The method for removing the silver plating layer of a lead frame according to claim 7, characterized in that: The deoxidation solution is 80 g / L to 120 g / L of sodium persulfate solution, and the soaking temperature is 30° C. to 40° C.

9. The method for removing the silver plating layer of a lead frame according to claim 1, characterized in that: Also includes: S4, placing the lead frame obtained in S3 in a protective aqueous solution at room temperature for anti-discoloration treatment, to obtain a lead frame with a partial silver plating layer removed.

10. A lead frame bonding method, characterized in that: include: The lead frame obtained by the lead frame silver plating removal method according to any one of claims 1 to 9 is bonded with a chip, cured and baked, one end of the bonding wire is bonded to the chip pad, and the other end of the bonding wire is bonded to the center of the silver plating bonding area on the lead frame.