Method for preparing coating liquid for secondary battery cathode comprising carbon-based nanocomposite
By using carbon nanocomposite coating liquid in lithium-ion batteries, the capacity reduction problem caused by volume expansion of silicon material is solved, the capacity expansion and energy density of secondary batteries are achieved, and the electrochemical performance of the battery is significantly improved. stability.
Patent Information
- Application Number
- CN202411026322.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-05
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing cathode active substance of silicon materials for lithium-ion batteries has caused volume expansion problems caused by lithium embedding, resulting in reduced battery capacity and safety risks, and traditional solutions have failed to effectively improve energy density.
Using a composite coating solution with encapsulated carbon nanocomposites, silicon nanoparticles are prepared, surface-treated carbon nanostructures and mixed with binder to form a structure of carbon nanotubes wrapped in silicon particles, combined with conductive metal-expanding Graphite composite, prepare coating solution for cathode of secondary battery to improve battery capacity and energy density.
The capacity expansion of secondary battery and the energy density are achieved, the volume expansion rate is reduced, and the electrochemical stability and charging and discharge characteristics of the battery are improved.
Smart Images

Figure CN118969969A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a coating liquid for a secondary battery cathode comprising a carbon nanocomposite. Background Art
[0002] When artificial graphite is used as a cathode active material for lithium-ion batteries instead of natural graphite, the structural stability can be further improved. Therefore, artificial graphite has been used more recently, but it has the disadvantage of being more expensive than natural graphite. Although the short-term prospect is to use graphite as a cathode active material, if it approaches 372mAh / g, which is the theoretical storage capacity, it will reach the limit value where the battery's charging capacity cannot be further increased. Therefore, in order to overcome such problems, research on new cathode active materials is being actively carried out. As mentioned above, since the cathode active material has reached the limit that determines the performance limit of lithium-ion batteries, it is important that the characteristics of the material itself and the morphology when formed in the electrode will also have a greater impact on the capacity and performance of the battery. One of the attempts to increase the storage capacity of lithium is to replace silicon material as a cathode active material. In the past, graphite was a structure of 6 carbon atoms and 1 lithium atom combined to form LiC6. In comparison, Li22Si5, which is a structure with a maximum of 22 lithium atoms combined on 5 silicon atoms at 415°C, can theoretically have a capacity of 4200mAh / g, which is nearly 11 times that of graphite, and has received more attention. However, the problem is that there is a serious problem that the volume expansion (Swelling) of silicon caused by lithium embedding increases to 310% compared to the initial state. This will cause the battery to swell and release the diaphragm, thereby causing battery safety issues. Of course, at room temperature, Li15Si4 is composed of a structure of 15 lithium atoms combined on 4 silicon atoms, so that the volume expansion at this time is slightly reduced compared to high temperature, but there is still a 280% volume expansion. In addition, as lithium escapes, the volume shrinks and breaks, resulting in a rapid decrease in storage capacity. In order to solve this problem, although various solutions such as silicon oxide method and using carbon to coat silicon have been proposed and studied, the problem that the energy density of the original silicon is reduced has not been solved.
[0003] Prior Art Literature
[0004] Patent Literature
[0005] (Patent Document 1) (Prior Document 1) Korean Patent Publication No. 10-2572352B1 (August 24, 2023)
[0006] (Patent Document 2) (Prior Document 2) Korean Patent Publication No. 10-1896103B1 (August 31, 2018) Summary of the invention
[0007] Technical problems to be solved
[0008] The object of the present invention is to provide a coating liquid for a secondary battery cathode comprising a carbon nanocomposite and a method for preparing the same, which uses a composite coating liquid encapsulated with a carbon nanocomposite to achieve the effect of increasing the capacity and energy density of the secondary battery.
[0009] Technical solutions to solve problems
[0010] The coating liquid for secondary battery cathode including carbon nanocomposite of the present invention comprises: step a), preparing carbon nanocomposite; step b), preparing composite dispersion liquid including carbon nanotubes and conductivity additive; and step c), mixing the carbon nanocomposite in the composite dispersion liquid to prepare composite coating liquid.
[0011] The step a) comprises: step a-1), preparing silicon nanoparticles; step a-2), adding a surface treatment agent to a carbon nanomaterial to prepare a surface-treated carbon nanostructure; and step a-3), adding the surface-treated carbon nanostructure and a binder to the silicon nanoparticles and then grinding.
[0012] In the step a-3), milling is performed after the conductive metal-expanded graphite composite particles are added.
[0013] The particle size of the silicon nanoparticles in step a-1) is 0.1-150 nm.
[0014] The carbon nanotube is at least one selected from single-walled carbon nanotube (SWNT), double-walled carbon nanotube (DWNT), thin multi-walled carbon nanotube (thin multi-walled carbon nanotube) or multi-walled carbon nanotube (MWNT).
[0015] The conductive additive includes one selected from the group consisting of polyacrylic acid, polyacrylate, polymethacrylic acid, polymethyl methacrylate, polyacrylamide, polyvinyl acetate, polymaleic acid, polyethylene glycol, and polyimide.
[0016] The conductive metal is aluminum.
[0017] The present invention provides a coating liquid prepared by any one of the above-mentioned preparation methods.
[0018] Technical Effects
[0019] The present invention has the effect of increasing the capacity and energy density of a secondary battery by applying a composite coating liquid in which a carbon-based nanocomposite is encapsulated to a coating target substance to prepare a cathode. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of a method for preparing a coating liquid for a secondary battery cathode according to an embodiment of the present invention. DETAILED DESCRIPTION
[0021] The following is a more detailed description with reference to specific embodiments of the present invention. However, this is not intended to limit the present invention to a specific embodiment, but should be understood to cover all changes, equivalents and even substitutes included in the concept and technical scope of the present invention. In the process of describing the present invention, if it is determined that the specific description of the relevant known technology confuses the gist of the present invention, the detailed description thereof will be omitted.
[0022] The coating liquid for the cathode of a secondary battery of the present invention comprises: a) a step of preparing a carbon nanocomposite; b) a step of preparing a composite dispersion liquid comprising carbon nanotubes and a conductive additive; and c) a step of mixing the carbon nanocomposite into the composite dispersion liquid to prepare a composite coating liquid.
[0023] By going through the process from step a) to step c), there is an effect of promoting the capacity expansion and energy density increase of the secondary battery.
[0024] The step a) includes the following steps for preparation: a-1) the step of preparing silicon nanoparticles; a-2) the step of adding a surface treatment agent to a carbon-based nanomaterial to prepare a surface-treated carbon nanostructure; a-3) the step of adding the surface-treated carbon nanostructure and additives to the silicon nanoparticles and then milling.
[0025] First, the silicon nanoparticles of step a-1) are prepared by a ball milling process, which is a process for minimizing volume expansion caused by lithium ion penetration of silicon.
[0026] At this time, the particle size of the silicon nanoparticles in step a-1) is 0.1 to 150 nm.
[0027] Wherein, the particle size of the silicon nanoparticles can be 0.1 to 150nm, preferably 0.5 to 120nm, more preferably 0.8 to 100nm, and most preferably 1 to 90nm. At this time, if the particle size of the silicon nanoparticles is less than 0.1nm, the charging and discharging efficiency may be reduced due to the small particle size. On the contrary, if it is greater than 150nm, a large amount of lithium ions are inserted into a particle when the secondary battery is charged, and there is a problem of increasing the volume, and when discharging, a large amount of lithium ions escape and generate gaps, and there is a problem of causing cracks. At the same time, as the lithium ions are broken due to repeated charging and discharging, an SEI layer will be formed and the movement of electrons will no longer occur, which may result in a sharp decrease in the capacity of the lithium ion battery. That is, the electrode stability may be sharply reduced.
[0028] In addition, in the case of adding a surface treatment agent to the carbon-based nanomaterial to prepare a surface-treated carbon nanostructure in step a-2), the carbon nanotubes are surface-modified under the action of the surface treatment agent, so that hydroxyl groups (-OH) or carboxyl groups (-COOH) and functional groups as a combination of these groups may exist on their surfaces.
[0029] At this time, in the step a-2), the surface treatment agent can be one or more of sulfuric acid, nitric acid, phosphoric acid, hydrochloric acid, and hydrogen peroxide water, and preferably a mixed solution of sulfuric acid and nitric acid can be used. In addition, in order to improve the dispersibility of carbon nanotubes, ultrasonic treatment and stirring processes can be used.
[0030] At this time, the stirring process may be performed at a stirring speed of 1000 rpm or less, so that the hydrophilized carbon fibers are uniformly dispersed.
[0031] The stirring speed may be below 1000 rpm, below 800 rpm, or below 700 rpm.
[0032] In addition, by grinding after adding the surface-treated carbon nanostructure and the binder in the silicon nanoparticles through step a-3), a carbon-based nanocomposite is formed. By uniformly distributing the surface-treated carbon nanostructure on the silicon particle surface under the action of the binder in step a-2), an excellent electron conduction network can be formed between the silicon particle and the collector, thereby having the effect of being able to contribute to the improvement of the output characteristics, life characteristics, etc. of the battery.
[0033] At this time, the binder can be selected from the group consisting of epoxy resin, styrene-butadiene rubber, acrylated styrene-butadiene rubber, cyanoethylene-butadiene rubber, acrylic rubber, butyl rubber, ethylene-propyl copolymer, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl pyridine, chlorosulfonated polyethylene, perfluorosulfonic acid (nafion), polyester resin, acrylic resin, phenolic resin, polyvinyl alcohol resin, acrylic ester resin, polyaniline, polythiophene, polyacetylene, polypyrrole and PEDOT, and the most preferred is epoxy resin.
[0034] That is, the carbon-based nanocomposite formed through step a-1 to step a-3) has a shape in which silicon particles are wrapped by carbon nanotubes (carbon nanostructures).
[0035] Furthermore, the carbon-based nanocomposite can simultaneously achieve ion conductivity, electronic conductivity, and stability, and an electrochemical element using the carbon-based nanocomposite as a cathode can ensure excellent charge capacity and high charge and discharge characteristics.
[0036] In addition, in the step of preparing a composite dispersion liquid including carbon nanotubes and a conductive additive in step b), the carbon nanotubes are at least one selected from single-walled carbon nanotubes (SWNT), double-walled carbon nanotubes (DWNT), thin multi-walled carbon nanotubes (thin multi-walled carbon nanotubes) or multi-walled carbon nanotubes (MWNT). More preferably, in order to more firmly form a carbon nanotube layer on the surface of silicon particles, single-walled carbon nanotubes (SWNT) can be used, so that the carbon nanotube layer will not be easily detached even in the case of contraction and expansion of silicon during the driving of the battery. More preferably, in order to achieve the purpose of capacity expansion and increase in energy density of the present invention, the weight ratio of the carbon-based nanocomposite and the carbon nanotube is preferably 0.1:10 to 5:10. In the case of being composed of the above-mentioned weight ratio, it has the effect of improving dispersibility and conductivity.
[0037] The dispersed particle size of the single-walled carbon nanotubes is not particularly limited, but is preferably 1 to 15 μm. This is because if the dispersed particle size of the single-walled carbon nanotubes is less than 1 μm, it is difficult to uniformly cover the surface of the silicon particles or carbon nanocomposites as a whole, thereby causing the problem of excessively high contact resistance. If the dispersed particle size is greater than 15 μm, the dispersion stability of the composite coating liquid is reduced, thereby causing the problem of low reproducibility of resistance during coverage. In particular, in order to significantly reduce the powder resistance, the dispersed particle size of the single-walled carbon nanotubes is more preferably 3 to 10 μm.
[0038] The conductive additive includes one selected from the group consisting of polyacrylic acid, polyacrylate, polymethacrylic acid, polymethyl methacrylate, polyacrylamide, polyvinyl acetate, polymaleic acid, polyethylene glycol, and polyimide.
[0039] The content of the conductivity additive is not particularly limited, but is preferably 10 wt % or less, more preferably 0.1 to 5 wt % relative to the total weight of the composite coating liquid in order to minimize the increase in electrode resistance.
[0040] In the step a-3), the conductive metal-expanded graphite composite particles are added before milling.
[0041] The conductive metal is aluminum.
[0042] More specifically, the conductive metal-expanded graphite composite is a composite in which graphite is expanded in a carbon nanostructure, thereby embedding expanded graphite nanoplates having an ultra-thin plate thickness into aluminum particles. This composite not only has a high aspect ratio and a wide surface area, but also has good dispersibility and excellent mechanical properties, and thus has characteristics that are beneficial to increasing the charge capacity of a secondary battery.
[0043] In a state where the carbon nanostructure is uniformly distributed on the surface of the silicon particles, the conductive metal-expanded graphite composite is distributed at the bottom, inside, top, or multiple positions of the carbon nanostructure coating, and can be integrated with the carbon nanostructure. That is, since the carbon nanostructure and the conductive metal-expanded graphite composite are doped on the surface of the silicon particles, the electrochemical stability is improved and the charge capacity is increased.
[0044] According to the method, the step b) may further include a graphite composite to prepare a composite dispersion.
[0045] At this time, the graphite composite is equivalent to a composite obtained by mixing natural graphite, artificial graphite and an adhesive and then subjecting it to heat treatment. In the case of natural graphite, it exhibits expansion phenomena corresponding to a high degree of orientation or disadvantages in rapid charging performance, and has relatively more functional groups on the surface than artificial graphite, so there is a problem of poor high temperature characteristics. In view of this, by subjecting natural graphite, artificial graphite and an adhesive to heat treatment after mixing, the artificial graphite precursor can be artificially graphitized, and a graphite composite in which the functional groups of natural graphite are effectively removed can be obtained, thereby improving the capacity and life characteristics of the secondary battery.
[0046] The present invention can provide a coating liquid prepared by any of the above-mentioned preparation methods. The coating liquid can be applied to the surface of a coating object and then used after a drying process.
[0047] Hereinafter, the secondary battery cathode coating liquid according to a preferred embodiment of the present invention will be described in more detail. However, the scope of the present invention is not limited to the following embodiments.
[0048] Example 1
[0049] Preparation of silicon nanoparticles
[0050] (a-1) Silicon nanoparticles with a size of 150 nm or less are obtained by ball milling silicon powder.
[0051] Preparation of surface treated carbon nanostructures
[0052] (a-2) After adding 1 wt% of carbon nanotubes (MWCNT) to a mixed solution prepared by 8M sulfuric acid and nitric acid at a volume ratio of 3:1 (75 / 25, v / v), an ultrasonic treatment process was performed for 20 minutes, and then stirred at 80°C and 600 rpm in an overhead stirrer for 2 hours. Then, after filtering and washing, it was dried in a vacuum oven at 80°C for 48 hours to obtain a carbon nanostructure.
[0053] Preparation of Carbon Nanocomposites
[0054] (a-3) A carbon nanostructure and an epoxy resin were added to silicon nanoparticles and then ball-milled to prepare a carbon nanocomposite in which silicon particles were encapsulated by the carbon nanostructure. The silicon nanoparticles, the carbon nanostructure and the epoxy resin were mixed at a weight ratio of 10:5:1.
[0055] b) 2 wt % of 10 μm single-walled carbon nanotubes, 5 wt % of polyacrylic acid, 10 wt % of graphite, and the remaining amount of water were mixed to prepare a composite dispersion.
[0056] c) The carbon nanocomposite prepared in step a) is mixed with the composite dispersion liquid to prepare a composite coating liquid. In this case, the carbon nanocomposite is added so that its content is 10 wt % relative to the composite dispersion liquid composition.
[0057] Example 2
[0058] The preparation was carried out in the same manner as in Example 1, except that the aluminum particles (97 vol%) and the expanded graphite nanoplates (3 vol%) were dried at 100° C. and then ball-milled at 400 rpm, thereby further adding composite particles in which expanded graphite was embedded in the aluminum particles to the step a-3). At this time, the silicon nanoparticles, the carbon nanostructure, the composite particles, and the epoxy resin were mixed in a weight ratio of 10:5:2:1.
[0059] Example 3
[0060] Preparation is performed in the same manner as in Example 2, except that in step b), 5 wt% of a graphite composite is further included, and the graphite composite is prepared by mixing spherical natural graphite, coke, and a binder in a weight ratio of 1:1:0.1 and then heat-treating the mixture at 200°C to 300°C.
[0061] Comparative Example 1
[0062] 97 wt % of a silicon-based cathode active material (SiOx), 1 wt % of single-walled carbon nanotubes, and 2 wt % of a binder (styrene butadiene rubber) were mixed and stirred to prepare a secondary battery cathode coating liquid.
[0063] Experimental example
[0064] The cathode film was prepared by applying the coating solution prepared by the embodiments 1 to 3 and the comparative example 1 to the copper collector at a level of 60 μm. The cathode formed with the final film was compressed by a heated roller press to control the electrode density to 1.6 g / cc. Lithium secondary batteries using the cathodes prepared as described above were made and the characteristics of the lithium secondary batteries were evaluated. Table 1 below is a table showing the characteristics of lithium secondary batteries using the cathode materials of embodiments 1 to 3 and comparative example 1.
[0065] Table 1
[0066]
[0067] As shown in Table 1, when the carbon-based nanocomposite was used as in Examples 1 to 3, a higher charge-discharge capacity was exhibited and a higher capacity per electrode volume was obtained compared to when silicon not subjected to surface modification was used.
[0068] Furthermore, when the aluminum-expanded graphite composite is used as the particles, compared with the case of using only the carbon-based nanocomposite, the particles exhibit characteristics such as being able to maintain charge and discharge capacity characteristics and capacity retention rate for a long period of time and significantly reducing the volume expansion rate.
[0069] Although the above description is made through the limited embodiments of the present invention, the present invention is not limited thereto, and ordinary technicians in the technical field to which the present invention belongs can make various modifications and variations within the equivalent scope of the technical concept of the present invention and the attached claims.
Claims
1. A method for preparing a coating liquid for a secondary battery cathode, characterized in that: include: Step a), preparing a carbon nanocomposite; Step b), preparing a composite dispersion comprising carbon nanotubes and a conductivity additive; and Step c), mixing the carbon nanocomposite into the composite dispersion to prepare a composite coating liquid, The step a) comprises: Step a-1), preparing silicon nanoparticles; Step a-2), adding a surface treatment agent to the carbon nanomaterial to prepare a surface-treated carbon nanostructure; and Step a-3), adding the surface treated carbon nanostructure and a binder to the silicon nanoparticles and then grinding them.
2. The method for preparing a coating liquid for a secondary battery cathode according to claim 1, characterized in that: In the step a-3), milling is performed after the conductive metal-expanded graphite composite particles are added.
3. The method for preparing a coating liquid for a secondary battery cathode according to claim 1, characterized in that: The particle size of the silicon nanoparticles in step a-1) is 0.1-150 nm.
4. The method for preparing a coating liquid for a secondary battery cathode according to claim 1, characterized in that: The carbon nanotube is at least one selected from single-walled carbon nanotubes, double-walled carbon nanotubes, thin multi-walled carbon nanotubes or multi-walled carbon nanotubes.
5. The method for preparing a coating liquid for a secondary battery cathode according to claim 1, characterized in that: The conductivity additive includes polyacrylic acid, graphite and water.
6. The method for preparing a coating liquid for a secondary battery cathode according to claim 2, characterized in that: The conductive metal is aluminum. 7 . A coating liquid prepared by the method for preparing a coating liquid for a secondary battery cathode according to claim 1 .