Negative plate, lithium ion battery and preparation method
By using a hybrid negative electrode sheet of titanium niobium oxide and lithium titanate in lithium-ion batteries, the problems of short life and low energy density of the negative electrode materials of existing lithium-ion batteries are solved, and higher electrochemical performance and longer Battery life, suitable for new energy applications.
Patent Information
- Application Number
- CN202410767649.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium-ion battery anode materials have problems such as short life, low energy density and high cost in new energy applications such as electric vehicles, which limits their wide application.
Using a mixed negative electrode sheet including titanium niobium oxide and lithium titanate, a first active coating and a second active coating are coated on both sides of the current collector, combined with a conductive agent and a binder, a high capacity is prepared. High voltage and long life negative electrode plate.
It improves the comprehensive performance of lithium-ion batteries, including higher capacity and energy density, extends battery life, and simplifies the preparation process, allowing the batteries to show better electrochemical performance in new energy applications.
Smart Images

Figure CN118969976A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of batteries, and in particular relates to a negative electrode sheet, a lithium ion battery and a preparation method thereof. Background Art
[0002] With the development of science and technology and the penetration of environmental protection concepts, lithium-ion batteries have grown rapidly. Their applications range from mobile phones, Bluetooth, and computer batteries to new energy vehicles, energy storage systems, and power supply systems. Lithium-ion batteries have become one of the new generation of new energy. With the development of the new energy industry, the performance requirements for batteries are getting higher and higher.
[0003] At present, the negative electrodes of lithium-ion batteries on the market are mostly carbon materials such as graphite and hard carbon, which have high capacity and high energy density, but their lifespan is relatively short, reaching a maximum of thousands of times; lithium titanate negative electrode materials have the advantages of high safety, wide temperature range and long life, but their capacity and energy density are relatively low and their cost price is high, which limits their widespread application in new energy industries such as electric vehicles and start-stop. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a negative electrode sheet, a lithium ion battery and a preparation method thereof.
[0005] To achieve the above object, the technical solution adopted in the present invention is:
[0006] A negative electrode sheet comprises a current collector and a first active coating and a second active coating respectively coated on both sides of the current collector; the first active coating comprises titanium niobium oxide, and the second active coating comprises lithium titanate.
[0007] The titanium niobium oxide is TiNb2O7, Ti2Nb 10 O 29 One or a mixture of the two; the lithium titanate is Li4Ti5O 12。
[0008] The first active coating and the second active coating further independently include a conductive agent and a binder;
[0009] Preferably, the mass ratio of titanium niobium oxide, conductive agent and binder in the first active coating is: (90-98): (1-5): (1-5);
[0010] Preferably, the mass ratio of lithium titanate, conductive agent and binder in the second active coating is: (90-98): (1-5): (1-5);
[0011] Preferably, the conductive agent is any one or more of carbon black, graphite, acetylene black, nano-carbon fiber, and carbon nanotube;
[0012] Preferably, the binder is PVDF.
[0013] The current collector is copper foil, copper mesh, aluminum foil, aluminum mesh, coated aluminum foil, or perforated aluminum foil; preferably, the thickness of the current collector is 8 μm-20 μm.
[0014] The present invention also includes a method for preparing the negative electrode sheet, comprising the following steps: 1) independently preparing a first active coating slurry and a second active coating slurry; 2) applying the first active coating slurry and the second active coating slurry to both sides of the current collector respectively, drying, and rolling to obtain a negative electrode sheet.
[0015] The specific steps of step 1) are: independently mixing the components in the first active coating and the second active coating slurry according to the mass ratio, adding solvent to adjust the solid content to 35% to 55%, the viscosity to 3000mPa·s to 8000mPa·s, and the fineness to less than 50μm.
[0016] In step 2), the first active coating slurry and the second active coating slurry are independently coated with a density of 4 mg / cm 2 ~16mg / cm 2 ;
[0017] Preferably, the coating densities of the first active coating and the second active coating are different;
[0018] Preferably, the ratio of the coating density of the first active coating layer to that of the second active coating layer is 0.4-1.2.
[0019] Step 2) wherein the compaction density is 1.8-3.0 g / cm3; the thickness of the first active coating after compaction is 15-60 μm;
[0020] The thickness of the second active coating is 20-82 μm.
[0021] The present invention also includes a lithium ion battery, comprising the negative electrode sheet, the positive electrode sheet, the separator and the electrolyte;
[0022] Preferably, the positive electrode sheet is prepared by the following method: coating the positive electrode slurry prepared from the positive electrode active material on both sides of the positive electrode current collector, drying, and rolling to obtain the positive electrode sheet;
[0023] Preferably, the positive electrode active material is lithium manganese oxide, lithium cobalt oxide, ternary material, or lithium iron phosphate;
[0024] Preferably, the coating density of the positive electrode slurry on both sides of the positive electrode current collector is the same;
[0025] Preferably, the coating density is 2 mg / cm 2 ~28mg / cm 2.
[0026] The present invention also includes a method for preparing the lithium-ion battery, comprising the following steps: the first active coating and the second active coating in the negative electrode sheet are randomly aligned with the two sides of the positive electrode sheet, with a separator in the middle, and then the sheets are wound or stacked and assembled, and then an electrolyte is added to encapsulate the lithium-ion battery.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The structure of the titanium niobium oxide described in the negative electrode sheet of the present application is similar to that of lithium titanate, and is a spinel structure, with the advantages of high capacity, high voltage, and long life. It is distributed on both sides of the current collector with lithium titanate, so that the hybrid lithium titanate battery combines the advantages of high power, long life, and wide temperature range of lithium titanate batteries and the advantages of high capacity, high energy density, and high power of titanium niobium oxide. Compared with pure lithium titanate batteries, it has better electrochemical properties and further improves performance such as capacity and energy density. The preparation process of the hybrid lithium titanate negative electrode sheet is simple and easy to industrialize, and the battery containing the hybrid lithium titanate negative electrode sheet has more excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic diagram showing a negative electrode sheet according to an embodiment of the present invention;
[0030] Figure 2 A schematic diagram showing a positive electrode sheet according to an embodiment of the present invention;
[0031] Figure 3 A schematic diagram showing a lithium-ion battery according to an embodiment of the present invention; Figure 4 This is a schematic diagram of the discharge performance of a battery in Example 1 of the present invention; Figure 5 This is a schematic diagram of the discharge performance of the battery in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0033] Example 1
[0034] Figure 1 A negative electrode sheet is shown, comprising a current collector 10 and a first active coating 11 and a second active coating 12 respectively coated on both sides of the current collector; the first active coating comprises titanium niobium oxide, and the second active coating comprises lithium titanate.
[0035] The first active coating and the second active coating further independently include a conductive agent and a binder;
[0036] Preferably, the mass ratio of titanium niobium oxide, conductive agent and binder in the first active coating is: (90-98): (1-5): (1-5); specifically, it can be 90:5:5, 94:2:1, 98:1:1;
[0037] Preferably, the mass ratio of lithium titanate, conductive agent and binder in the second active coating is: (90-98): (1-5): (1-5); specifically, it can be 90:5:5, 94:2:1, 98:1:1;
[0038] Preferably, the conductive agent is any one or more of carbon black, graphite, acetylene black, nano-carbon fiber, and carbon nanotube; preferably, the binder is PVDF.
[0039] The current collector is copper foil, copper mesh, aluminum foil, aluminum mesh, coated aluminum foil, or perforated aluminum foil; preferably, the thickness of the current collector is 8 μm-20 μm, specifically 8 μm, 10 μm, 12 μm, 15 μm, or 20 μm.
[0040] The present invention also includes a method for preparing the negative electrode sheet, comprising the following steps: 1) independently preparing a first active coating slurry and a second active coating slurry; 2) applying the first active coating slurry and the second active coating slurry to both sides of the current collector respectively, drying, and rolling to obtain a negative electrode sheet.
[0041] The specific steps of step 1) are: independently mixing the components in the first active coating and the second active coating slurry according to the mass ratio, adding a solvent to adjust the solid content to 35% to 55%, the viscosity to 3000mPa·s to 8000mPa·s, and the fineness to be less than 50μm. Specifically, the solid content can be 35%, the viscosity can be 3000mPa·s; or the solid content can be 55%, and the viscosity can be 8000mPa·s;
[0042] In step 2), the first active coating slurry and the second active coating slurry are independently coated with a density of 4 mg / cm 2 ~16mg / cm 2 ; Specifically, it can be 4mg / cm 2 、10mg / cm 2 、16mg / cm 2 etc;
[0043] Preferably, the coating densities of the first active coating and the second active coating are different;
[0044] Preferably, the coating density ratio of the first active coating layer to the second active coating layer is 0.4-1.2. Specifically, it can be 0.4, 0.78, or 1.2;
[0045] Step 2) Compacted density 1.8-3.0g / cm 3 ; Specifically, it can be 1.8g / cm3, 2.0g / cm3, 2.3g / cm3, 3.0g / cm3; the thickness of the first active coating after compaction is 15-60μm. Specifically, it can be 15μm, 40μm, 60μm.
[0046] The thickness of the second active coating layer is 20-82 μm, specifically 20 μm, 60 μm, or 82 μm.
[0047] The present invention also includes a lithium ion battery, comprising the negative electrode sheet, the positive electrode sheet, the separator and the electrolyte;
[0048] Preferably, the positive electrode sheet is prepared by the following method: coating the positive electrode slurry prepared from the positive electrode active material on both sides of the positive electrode current collector, drying, and rolling to obtain the positive electrode sheet;
[0049] Preferably, the positive electrode active material is lithium manganese oxide, lithium cobalt oxide, ternary material, or lithium iron phosphate;
[0050] Preferably, the coating density of the positive electrode slurry on both sides of the positive electrode current collector is the same; preferably, the coating density is 2 mg / cm 2 ~28mg / cm 2 . Specifically, it can be 2mg / cm 2 、12.37mg / cm 2 、28mg / cm 2 .
[0051] The present invention also includes a method for preparing the lithium-ion battery, comprising the following steps: the first active coating and the second active coating in the negative electrode sheet are randomly aligned with the two sides of the positive electrode sheet, with a separator in the middle, and then the sheets are wound or stacked and assembled, and then an electrolyte is added to encapsulate the lithium-ion battery.
[0052] The following is described with specific embodiments:
[0053] Example 1
[0054] The preparation method of the negative electrode sheet specifically includes the following steps: a first active coating slurry is prepared by mixing titanium niobium oxide TiNb2O7, a conductive agent, and a binder in a ratio of 94:4:2, wherein the conductive agent comprises SP and CNT (the ratio of the two is 2:1), and a solvent NMP is added to adjust the viscosity to 5000 mPa·s and the fineness to 30 μm to prepare a first negative electrode slurry, which is coated on a 12 μm aluminum foil current collector, and the single-sided coating surface density is 9.35 mg / cm 2 , after drying, a single-sided electrode is obtained;
[0055] The second active coating slurry is composed of lithium titanate Li4Ti5O 12 The conductive agent and the binder are mixed in a ratio of 94:4:2. The conductive agent includes SP and CNT (the ratio of the two is 2:1). The conductive agent is prepared by stirring and mixing. The solvent NMP is added to adjust the viscosity to 5300mPa·s and the fineness to 30μm to obtain the second negative electrode slurry, which is coated on the other side of the 12μm aluminum foil current collector. The single-sided coating surface density is 12mg / cm 2 After drying, a mixed electrode is obtained.
[0056] In addition to the above method of single-layer coating of two materials, a double-sided coating device can also be used to directly coat two different negative electrode slurries on both sides of the aluminum foil, and then a mixed electrode can be directly obtained by drying the mixed electrode.
[0057] In this embodiment, the ratio of the coating density of the first active coating layer to that of the second active coating layer is 0.78.
[0058] The obtained negative electrode sheet was roll-pressed, and the compaction density was 2.28 g / cm 3 The thickness of the negative electrode sheet after rolling is 106μm.
[0059] The preparation method of the positive electrode sheet is similar to that of the negative electrode sheet. The positive electrode active material is lithium cobalt oxide material, and its single-sided coating surface density is 12.37 mg / cm 2 The compacted density is 3.8g / cm 3 The current collector is 12 μm aluminum foil, and the thickness of the electrode after rolling is 77 μm. The obtained positive electrode is as follows Figure 2 As shown, it includes a positive electrode current collector 20 and a positive electrode active layer coated on both sides of the current collector; the positive electrode active layer includes a first positive electrode active layer 21 and a second positive electrode active layer 22.
[0060] Then, the obtained positive electrode sheet and negative electrode sheet are assembled into a battery ( Figure 3 As shown, the first active coating 11 and the second active coating 12 in the negative electrode sheet correspond to the positive electrode sheet in the direction that the first active coating 11 of the negative electrode faces the first positive electrode active layer 21, and the second active coating of the negative electrode faces the second positive electrode active layer 22, with a separator in the middle. After assembly, an electrolyte is added to encapsulate to obtain a lithium-ion battery, and its discharge performance schematic diagram is shown as follows Figure 4 .
[0061] Example 2
[0062] The preparation of the positive and negative electrode sheets in Example 2 is the same as that in Example 1, with the only difference being that, during the assembly process, the corresponding relationship between the positive and negative electrode sheets is different, the first active coating 11 of the negative electrode sheet is opposite to the second positive electrode active layer 22, and the second active coating 11 of the negative electrode sheet is opposite to the first positive electrode active layer 21 of the positive electrode sheet, and the other assembly processes are the same. Since the active materials of the coatings on both sides of the positive electrode sheets in this application are consistent, the results are similar to those in Example 1.
[0063] Example 3
[0064] The preparation of the negative electrode sheet in Example 3 is different from that in Example 1 in that the first active coating slurry is a mixture of Ti Nb2O7, a conductive agent, and a binder in a ratio of 96:2:2, and the second active coating slurry is a mixture of LTO, a conductive agent, and a binder in a ratio of 96:2:2.
[0065] The other processes are the same as those in Example 1.
[0066] Example 4
[0067] The preparation of the negative electrode sheet in Example 4 is different from that in Example 1 in that the coating surface density of the negative electrode is changed. The single-sided coating surface density of the first active coating of the negative electrode sheet is 8 mg / cm 2 The second active coating has a single-sided coating density of 10.25 mg / cm 2 The compacted density is 2.28g / cm 3 The thickness of the negative electrode sheet after rolling is 92 μm, and the ratio of the coating density of the first active coating layer to the second active coating layer is still 0.78.
[0068] The positive electrode is made of lithium cobalt oxide material, and its single-sided coating surface density is 10.57 mg / cm 2 The compacted density is 3.8g / cm 3 The current collector is 12μm aluminum foil, and the thickness of the electrode after rolling is 68μm.
[0069] The other processes are the same as those in Example 1.
[0070] Example 5
[0071] The preparation of the negative electrode sheet in Example 5 is different from that in Example 1 in that the coating density ratio of the first active coating layer and the second active coating layer of the negative electrode is changed to 0.7, and the single-sided coating density of the first active coating layer of the negative electrode sheet is 8.35 mg / cm 2 The second active coating has a single-sided coating density of 12 mg / cm 2 The compacted density is 2.28g / cm 3 The thickness of the negative electrode sheet after rolling is 102μm.
[0072] The positive electrode is made of lithium cobalt oxide material, and its single-sided coating density is 12.37 mg / cm2 The compacted density is 3.8g / cm 3 The current collector is 12μm aluminum foil, and the thickness of the electrode after rolling is 77μm.
[0073] The other processes are the same as those in Example 1.
[0074] Comparative Example 1
[0075] The difference between Comparative Example 1 and Example 1 is that both sides of the negative electrode sheet are coated with the second active coating: the negative electrode sheet is prepared by mixing the second active coating slurry with lithium titanate, conductive agent and binder in a ratio of 94:4:2 and stirring, and the single-sided coating surface density of this negative electrode slurry is 12 mg / cm 2 After adding solvent NMP to adjust the viscosity to 5300mPa·s and the fineness to 30μm, it was coated on both sides of the 12μm aluminum foil current collector and dried to obtain the lithium titanate pole piece.
[0076] The obtained pole piece was rolled and the compaction density was 1.95 g / cm 3 The thickness of the electrode sheet after rolling is 135 μm. The assembly process is the same as that of Example 1. The discharge performance diagram is shown in Figure 5 .
[0077] Comparative Example 2
[0078] The difference between Comparative Example 2 and Example 1 is that both sides of the negative electrode sheet are coated with a mixed coating of the first active slurry and the second active slurry; the active materials TiNb2O7 and LTO of the negative electrode sheet are mixed in a ratio of 43.8:56.2, and then the mixed active material, conductive agent, and binder are mixed in a ratio of 94:4:2, and the single-sided coating surface density of this negative electrode slurry is 10.68 mg / cm 2 After adding solvent NMP to adjust the viscosity to 5000mPa·s and the fineness to 30μm, it was coated on both sides of the 12μm aluminum foil current collector and dried to obtain the lithium titanate pole piece.
[0079] The obtained pole piece was roll-pressed, and the compaction density was 2.28 g / cm 3 The thickness of the negative electrode sheet after rolling is 106μm.
[0080] Table 1
[0081]
[0082]
[0083] Table 2
[0084] magnification 1C 2C 3C 5C 10C 15C 20C Example 1 96.4% 94.0% 93.0% 91.0% 87.8% 94.0% 80.5% Example 2 96.3% 94.3% 93.4% 91.1% 87.5% 94.1% 80.4% Example 3 96.0% 93.0% 92.2% 90.1% 87.0% 93.4% 79.3% Example 4 96.5% 94.3% 92.6% 91.3% 88.0% 94.0% 80.9% Example 5 96.3% 94.0% 93.0% 91.1% 87.5% 93.9% 80.0% Comparative Example 1 95.8% 92.8% 89.9% 84.9% 65.3% 39.8% 8.7% Comparative Example 2 96.0% 93.0% 91.1% 86.0% 73.0% 47.0% 30.0%
[0085] Table 3
[0086] magnification 1C 3C 5C 10C 15C 20C Example 1 100.0% 98.0% 97.0% 96.0% 95.0% 93.0% Example 2 100.0% 99.4% 97.5% 96.4% 95.2% 92.3% Example 3 100.0% 99.0% 97.2% 96.1% 94.9% 92.0% Example 4 100.0% 99.5% 97.6% 96.5% 95.8% 94.0% Example 5 100.0% 99.4% 97.3% 96.1% 95.5% 93.9% Comparative Example 1 100.0% 99.5% 97.3% 93.5% 82.5% 68.6% Comparative Example 2 100.0% 98.0% 97.0% 94.3% 85.0% 77.0%
[0087] Table 4
[0088] Battery ID type Cycle times Retention rate A3 Example 1 1000 99.0% B3 Example 2 1000 99.1% C3 Example 3 1000 99.0% D3 Example 4 1000 99.2% E3 Example 5 1000 99.2% Y3 Comparative Example 1 1000 99.1% Z3 Comparative Example 2 1000 98.9%
[0089] Table 5
[0090]
[0091]
[0092] The capacity data of the embodiment and comparative battery are shown in Table 1, wherein the capacity of embodiment 1 reaches 4.2Ah, and the energy density is as high as 95Wh / kg, which is 15% to 20% higher than comparative example 1 and about 5% higher than comparative example 2. The battery containing the mixed negative electrode sheet has a lower internal resistance, which is more than 50% lower than the internal resistance of the battery in comparative example 1 and about 20% lower than comparative example 2, reducing the heat generation of the battery during the high-rate charge and discharge process and improving the power performance of the battery. The charging power performance of the battery in embodiment 1 is excellent. In high-rate charging, it can reach more than 80% of the 20C constant current segment charging (Table 2), and the constant current and constant voltage charging reaches 100% of the capacity. The 20C constant current segment charging in comparative example 1 only reaches 8.7%, which is nearly 9 times higher. The 20C constant current segment charging in comparative example 2 reaches 30%, which greatly improves the rate charging performance of the battery.
[0093] As can be seen from Table 3, the battery containing the hybrid negative electrode sheet in Example 1 has excellent high-rate discharge performance. Under the condition of 20C high-rate discharge, the discharge capacity accounts for 93%, and the maximum discharge current can reach 50C. Under the same conditions, the pure lithium titanate battery in Example 1 has a 20C high-rate discharge, and its discharge capacity accounts for 68%, which improves the performance by 40%. The battery in Example 2 has a 20C high-rate discharge, and its discharge capacity accounts for 77%, which improves by about 20%.
[0094] The cycle performance of the hybrid battery in Example 1 is similar to that of the conventional lithium titanate battery in Comparative Example 1. As shown in Table 4, the capacity retention rate of the battery after 1000 cycles is about 99%, and the gas production inside the battery is measured after the cycle. The gas production of the battery in Example 1 is relatively small (Table 5), which reduces the gas production of the battery prepared with pure lithium titanate negative electrode material.
[0095] Comparing the data of Example 1 and Example 2, the capacity, internal resistance and energy density of the two are almost the same, and there is little difference in the charge and discharge performance and cycle performance, which shows that the active materials on both sides of the negative electrode sheet and the positive electrode sheet can correspond randomly.
[0096] Example 3 changes the content of the negative electrode active material on the basis of Example 1, and increases the proportion of the active material from 94% to 96%. From Tables 1-3, it can be seen that the capacity and energy density are slightly increased, and the charge and discharge performance is not much different.
[0097] Example 5 changes the coating surface density of the negative electrode, reduces the coating surface density of the two negative electrode active materials, and the corresponding positive electrode coating surface density is also reduced. The overall thickness of the positive and negative electrodes is reduced, and the capacity and energy density of the battery are also reduced (as shown in Table 1), but its discharge performance is slightly increased compared with Example 1, but the magnitude is not large, and other performances are similar. Example 5 changes the coating density ratio of the first active coating layer and the second active coating layer of the negative electrode to 0.7, reduces the coating amount of TiNb2O7, and the coating density of other active materials remains unchanged. Finally, the battery capacity is slightly reduced, and the charge and discharge performance is not much different.
[0098] In summary, the battery containing the hybrid negative electrode sheet has a higher capacity and energy density than the pure lithium titanate battery, and also has excellent charging and discharging power performance, no gas production, and a long battery life. Compared with the traditional lithium titanate battery negative electrode sheet, the hybrid negative electrode sheet can be prepared by using a double-sided coating device to coat two different types of negative electrodes. The operation and preparation process are simple and easy to industrialize, and the battery containing the hybrid negative electrode sheet has excellent performance.
[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A negative electrode sheet, characterized in that: It comprises a current collector and a first active coating and a second active coating respectively coated on both sides of the current collector; the first active coating comprises titanium niobium oxide, and the second active coating comprises lithium titanate.
2. The negative electrode sheet according to claim 1, characterized in that: The titanium niobium oxide is TiNb2O7, Ti2Nb 10 O 29 One or a mixture of the two; the lithium titanate is Li4Ti5O 12。 3. The negative electrode sheet according to claim 1, characterized in that: The first active coating and the second active coating further independently include a conductive agent and a binder; Preferably, the mass ratio of titanium niobium oxide, conductive agent and binder in the first active coating is: (90-98): (1-5): (1-5); Preferably, the mass ratio of lithium titanate, conductive agent and binder in the second active coating is: (90-98): (1-5): (1-5); Preferably, the conductive agent is any one or more of carbon black, graphite, acetylene black, nano-carbon fiber, and carbon nanotube; Preferably, the binder is PVDF.
4. The negative electrode sheet according to claim 1, characterized in that: The current collector is copper foil, copper mesh, aluminum foil, aluminum mesh, coated aluminum foil, or perforated aluminum foil; preferably, the thickness of the current collector is 8 μm-20 μm.
5. A method for preparing a negative electrode sheet according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) independently preparing a first active coating slurry and a second active coating slurry; 2) coating the first active coating slurry and the second active coating slurry on both sides of the current collector respectively, drying, and rolling to obtain a negative electrode sheet.
6. The preparation method according to claim 5, characterized in that: The specific steps of step 1) are: independently mixing the components in the first active coating and the second active coating slurry according to the mass ratio, adding solvent to adjust the solid content to 35% to 55%, the viscosity to 3000mPa·s to 8000mPa·s, and the fineness to less than 50μm.
7. The preparation method according to claim 5, characterized in that: In step 2), the first active coating slurry and the second active coating slurry are independently coated with a density of 4 mg / cm 2 ~16mg / cm 2 ; Preferably, the coating densities of the first active coating and the second active coating are different; Preferably, the ratio of the coating density of the first active coating layer to that of the second active coating layer is 0.4-1.
2.
8. The preparation method according to claim 5, characterized in that: Step 2) Compacted density 1.8-3.0g / cm 3 ; The thickness of the first active coating after compaction is 20-82 μm; The thickness of the second active coating is 15-60 μm.
9. A lithium ion battery, characterized in that: Comprising the negative electrode sheet, positive electrode sheet, separator and electrolyte according to any one of claims 1 to 4; Preferably, the positive electrode sheet is prepared by the following method: coating the positive electrode slurry prepared from the positive electrode active material on both sides of the positive electrode current collector, drying, and rolling to obtain the positive electrode sheet; Preferably, the positive electrode active material is lithium manganese oxide, lithium cobalt oxide, ternary material, or lithium iron phosphate; Preferably, the coating density of the positive electrode slurry on both sides of the positive electrode current collector is the same; Preferably, the coating density is 2 mg / cm 2 ~28mg / cm 2 .
10. A method for preparing a lithium ion battery according to claim 9, characterized in that: The method comprises the following steps: the first active coating and the second active coating in the negative electrode sheet are randomly aligned with the two sides of the positive electrode sheet, with a separator in the middle, and then winding or stacking the sheets and adding electrolyte to encapsulate to obtain a lithium-ion battery.