Positive electrode material, secondary battery, and electric device
By coating a carbon layer on the surface of lithium iron manganese oxide and doping it with specific non-metallic elements, combined with lithium manganese oxide, the problems of manganese leaching and active lithium loss in lithium iron manganese oxide cathode materials are solved, improving the SOC-OCV curve shift of the battery and the difficulty of BMS management.
Patent Information
- Application Number
- CN202411027219.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Lithium iron manganese oxide cathode materials suffer from active lithium loss and manganese leaching during high-temperature cycling, resulting in a significant shift in the SOC-OCV curve and increased difficulty in BMS management at the end of the warranty period.
A carbon layer is coated on the surface of lithium iron manganese oxide and doped with group IIIA, VA or VIA nonmetallic elements, such as S, N, P, B, and used in combination with lithium manganese oxide to form an improved cathode material.
It effectively suppresses the degradation of the cyclic manganese platform, reduces the loss of active lithium, improves the SOC-OCV curve shift throughout the entire life cycle of the secondary battery, and reduces the difficulty of BMS management at the end of the warranty period.
Smart Images

Figure BDA0004969754220000111 
Figure BDA0004969754220000121
Abstract
Description
Technical Field
[0001] The present application relates to the field of positive electrode technology, in particular to a positive electrode material, a secondary battery and an electrical device. Background Art
[0002] Manganese iron lithium oxide is a type of positive electrode material with good safety and stability. On the basis of iron lithium oxide, manganese is added to increase the charging voltage, which can increase the energy density by more than 15%, and the cost is basically the same as that of iron lithium oxide. However, manganese iron lithium oxide suffers from a large amount of active lithium loss during high-temperature cycling, accompanied by serious manganese dissolution problems, which causes a serious deviation in the SOC-OCV curve of manganese iron lithium oxide batteries throughout their life cycle, which will cause problems with BMS management at the end of the warranty period. Summary of the invention
[0003] The purpose of the present application is to provide a positive electrode material, a secondary battery and an electrical device to improve the problem that the existing battery using manganese iron lithium oxide as the positive electrode material has a serious deviation in the SOC-OCV curve throughout the life cycle and is difficult to manage the BMS at the end of the warranty period.
[0004] To achieve the above-mentioned purpose, in the first aspect of the present application, a positive electrode material is provided, wherein the positive electrode material comprises lithium iron manganese oxide and lithium manganate, wherein at least a portion of the surface of the lithium iron manganese oxide has a carbon coating layer, wherein the carbon coating layer contains inorganic non-metallic elements, and the inorganic non-metallic elements include non-metallic elements in groups IIIA, VA or VIA.
[0005] As an embodiment of the present application, the inorganic non-metallic element includes at least one of S, N, P, and B.
[0006] As an embodiment of the present application, based on the total weight of the manganese iron lithium oxide, the content of the carbon coating layer is 1 wt % to 4 wt %.
[0007] As an implementation scheme of the present application, the weight percentage of lithium manganese oxide in the positive electrode material is n1%, satisfying: n1≥10.
[0008] As an implementation scheme of the present application, the weight percentage of lithium manganese oxide in the positive electrode material is n1%, satisfying: n1≥30.
[0009] As an embodiment of the present application, the molar ratio of manganese atoms to iron atoms in the manganese-iron lithium oxide is Mn / Fe≥1.
[0010] As an embodiment of the present application, the molar ratio Mn / Fe of manganese atoms to iron atoms in the manganese-iron lithium oxide is 7:3 to 9:1.
[0011] A second aspect of the present application provides a secondary battery, wherein the secondary battery comprises a positive electrode plate, and the positive electrode plate comprises the positive electrode material described in the first aspect of the present application.
[0012] As an embodiment of the present application, the compaction density of the positive electrode sheet is 2.36 to 3.05 g / cm 3 .
[0013] According to a third aspect of the present application, an electrical device is provided, wherein the electrical device comprises the secondary battery according to the second aspect of the present application.
[0014] Compared with the prior art, the beneficial effects of this application are:
[0015] The positive electrode material described in the present application includes lithium iron manganese oxide and lithium manganate, and at least part of the surface of the lithium iron manganese oxide has a carbon coating layer, and the carbon coating layer contains inorganic non-metallic elements, and the inorganic non-metallic elements include non-metallic elements in the IIIA, VA or VIA group. The present application improves the serious deviation of the SOC-OCV curve of the lithium iron manganese oxide secondary battery throughout its life cycle by mixing lithium manganese oxide with lithium iron manganese oxide and doping specific inorganic non-metallic elements into the carbon coating layer of the lithium iron manganese oxide, thereby reducing the difficulty of managing the BMS at the end of the warranty period. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0017] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0018] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0019] The reagents or instruments used in this application without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0020] An embodiment of the present application provides a positive electrode material, which includes manganese iron lithium oxide and lithium manganate, at least part of the surface of the manganese iron lithium oxide has a carbon coating layer, the carbon coating layer contains inorganic non-metallic elements, and the inorganic non-metallic elements include non-metallic elements in groups IIIA, VA or VIA.
[0021] In some embodiments, the inorganic non-metallic element includes at least one of S, N, P, and B. For example, the inorganic non-metallic element contained in the carbon coating layer may be S, N, P, B, S and B, S and N, S and P, N and P, N and B, or P and B. When the inorganic non-metallic element further includes the above elements, the decay of the cyclic manganese platform is suppressed, thereby further improving the problem of SOC-OCV curve deviation during the entire life cycle of the battery.
[0022] In some embodiments, based on the total weight of the manganese iron lithium oxide, the content of the carbon coating layer is 1wt% to 4wt%. For example, the content of the carbon coating layer can be any one of 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, or a range between any two values. When the content of the carbon coating layer is within the above range, it can suppress the decay of the cyclic manganese platform to a certain extent, while making the manganese iron lithium oxide have a higher gram capacity and compaction density, thereby improving the problem of SOC-OCV curve deviation during the entire life cycle of the battery and taking into account a higher energy density.
[0023] In some embodiments, the weight percentage of lithium manganese oxide in the positive electrode material is n1%, satisfying: n1 ≥ 10. For example, the weight percentage of lithium manganese oxide in the positive electrode material is any one of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or a range between any two values. When the weight percentage of lithium manganese oxide in the positive electrode material is within the above range, the battery manganese platform capacity accounts for a large proportion, and the iron platform attenuation caused by the loss of active lithium in the battery at the end of the cycle is reduced, thereby further improving the problem of SOC-OCV curve deviation over the entire life cycle of the secondary battery.
[0024] In some embodiments, the molar ratio of manganese atoms to iron atoms in the manganese iron lithium oxide is Mn / Fe≥1. For example, the molar ratio of manganese atoms to iron atoms in the manganese iron lithium oxide is Mn / Fe≥1. For example, the molar ratio of manganese atoms to iron atoms in the manganese iron lithium oxide is 5:5, 6:4, 7:3, 8:2, 9:1, or any range between any two values. When the molar ratio of manganese atoms to iron atoms in the manganese iron lithium oxide is Mn / Fe≥1, the problem of SOC-OCV curve deviation in the full life cycle of the secondary battery can be further improved.
[0025] In some embodiments, the average particle size of the manganese iron lithium oxide is smaller than the average particle size of the lithium manganate. The combination of manganese iron lithium oxide and lithium manganate can increase the overall compaction density of the obtained positive electrode material without reducing the compaction density of the manganese iron lithium oxide itself, thereby facilitating the improvement of the energy density of the secondary battery.
[0026] In some embodiments, the general formula of manganese iron lithium oxide includes Li a Mn x Fe 1-x PO4, wherein 0.95≤a≤1.05, 0.5≤x≤0.9, specifically, x includes any one of 0.5, 0.6, 0.7, 0.8, and 0.9. For example, manganese iron lithium oxide can be LiMn 0.5 Fe 0.5 PO4、LiMn 0.6 Fe 0.4 PO4、LiMn 0.7 Fe 0.3 PO4、LiMn 0.8 Fe 0.2 PO4、LiMn 0.9 Fe 0.1 Any one of PO4.
[0027] In a second aspect of the present application, a secondary battery is provided, comprising a positive electrode plate, wherein the positive electrode plate comprises a positive electrode collector and a positive electrode material layer arranged on at least one surface of the positive electrode collector, wherein the positive electrode material layer comprises the positive electrode material described in the first aspect of the present application.
[0028] In some embodiments, the compaction density of the positive electrode sheet is 2.36-3.05 g / cm 3 For example, the compaction density of the positive electrode sheet can be 2.36 g / cm 3 , 2.48g / cm 3 , 2.59g / cm 3 , 2.71g / cm 3 , 2.82g / cm 3 , 2.94g / cm 3 、3.05g / cm 3 Any value or range between any two values in .
[0029] The type of positive electrode current collector is not specifically limited and can be selected according to actual needs. Preferably, aluminum foil or carbon-coated aluminum foil can be used.
[0030] In some embodiments, the secondary battery further comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode material.
[0031] The type of negative electrode material is not specifically limited and can be selected according to actual needs. For example, the negative electrode material can be artificial graphite, natural graphite, silicon-carbon composite material, silicon oxide, hard carbon, lithium metal and lithium titanate.
[0032] The type of negative electrode current collector is not particularly limited and can be selected according to actual needs. Preferably, copper foil or carbon-coated copper foil can be used.
[0033] In some embodiments, the secondary battery further comprises a separator. The type of separator is not particularly limited and can be selected according to actual needs. The separator can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride, a spandex film, an aramid film, or a multilayer composite film modified by a coating.
[0034] In some embodiments, the preparation of a secondary battery includes: stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then winding them into a square bare cell, loading them into a battery casing, and then baking them at 65 to 95°C to remove water, injecting electrolyte, sealing, and obtaining a secondary battery after standing, hot and cold pressing, formation, clamping, capacity division and other processes.
[0035] In some embodiments, the secondary battery may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package, and the material of the soft package may be plastic, such as one or more of polypropylene, polybutylene terephthalate, polybutylene succinate, etc.
[0036] In some embodiments, the shape of the secondary battery is not particularly limited, and it can be cylindrical, square, or any other shape.
[0037] The third aspect of the present application provides an electric device, which includes the secondary battery described in the second aspect of the present application. The electric device can be an application device such as a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, and an electric tool. The vehicle can be a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and a railway electric tool, such as an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc. The embodiments of the present application do not impose any special restrictions on the above-mentioned devices.
[0038] The following are specific embodiments of the present application, and the technical scheme of the present application is further described in conjunction with the embodiments, but the present application is not limited to these embodiments. The reagents, methods and equipment used in the present application, unless otherwise specified, are conventional reagents, methods and equipment in the art.
[0039] Example 1
[0040] Embodiment 1 provides a secondary battery, and the specific preparation process of the secondary battery includes:
[0041] (1) Preparation of positive electrode materials
[0042] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0043] S2. The primary positive electrode active material, glucose and sublimed sulfur were weighed in a mass ratio of 80:15:5, a small amount of deionized water was added, high-energy ball milling was performed for 6 hours, drying was performed, and then sintering was performed at 550°C for 4 hours in an ammonia-argon mixed atmosphere (the volume fraction of ammonia was 5%) to obtain S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 3wt%.
[0044] S3. Prepared S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 9:1 to obtain a positive electrode material.
[0045] (2) Preparation of positive electrode sheet
[0046] The positive electrode material, conductive agent carbon black, and binder polyvinylidene fluoride are mixed in a mass ratio of 96.3:2:1.7, and then mixed and stirred with 1-methyl-2-pyrrolidone to obtain a positive electrode slurry, and then the positive electrode slurry is coated on both sides of the aluminum foil, and the positive electrode sheet is obtained through the processes of baking, rolling, slitting, and cutting.
[0047] (3) Preparation of negative electrode sheet
[0048] The negative electrode material graphite, the conductive agent carbon black, the dispersant CMC and the binder SBR are mixed in a mass ratio of 97:0.6:0.9:1.5, and deionized water is added to stir and disperse evenly at a high speed, and the slurry viscosity is adjusted to 4000cps to obtain a negative electrode slurry, and then the prepared negative electrode slurry is sieved with a 150-mesh double-layer filter cloth, extruded and coated on the upper and lower surfaces of a 4.5μm copper foil, dried, and then cold pressed, slit, and cut to obtain a negative electrode sheet;
[0049] (4) Preparation of electrolyte
[0050] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) are mixed in a volume ratio of 1.2:0.8:1 to obtain an organic solvent, the solute lithium salt is lithium hexafluorophosphate (LiPF6), and the above mixed organic solvent is added to prepare an electrolyte with a concentration of 1.2 mol / L.
[0051] (5) Isolation film
[0052] The isolation membrane is composed of a 7μm polyethylene-based film + a single-sided 2μm ceramic coating + a single-sided 5μm polyvinylidene fluoride organic coating.
[0053] (6) Preparation of secondary batteries
[0054] The prepared positive and negative electrode sheets and isolation film are assembled into a roll core by winding, and then transferred into an aluminum-plastic film; the finished battery is obtained through processes such as liquid injection, packaging, standing, formation, aging, and capacity division.
[0055] Embodiments 2 to 7
[0056] The difference between Examples 2 to 7 and Example 1 is that the LiMn 0.6 Fe 0.4 The weight ratios of PO4 and lithium manganate oxide are different, namely 8:2, 7:3, 6:4, 5:5, 4:6, and 3:7, as shown in Table 1.
[0057] Example 8
[0058] The difference between Example 8 and Example 3 is that steps S2 and S3 in the method for preparing the positive electrode material are different, specifically:
[0059] S2. The primary positive electrode active material, glucose, sublimed sulfur and boric acid were weighed in a mass ratio of 75:15:5:5, and a small amount of deionized water was added. The mixture was subjected to high-energy ball milling for 6 hours, dried, and then sintered at 550°C for 4 hours in an argon atmosphere to obtain S / B co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 material;
[0060] S3. Prepared S / B co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0061] Example 9
[0062] The difference between Example 9 and Example 3 is that steps S2 and S3 in the method for preparing the positive electrode material are different, specifically:
[0063] S2. The primary active material, glucose and boric acid were weighed in a mass ratio of 80:15:5, a small amount of deionized water was added, high-energy ball milling was performed for 6 hours, drying was performed, and then sintering was performed at 550°C for 4 hours in an ammonia-argon mixed atmosphere (the volume fraction of ammonia was 5%) to obtain B / N co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 material;
[0064] S3. Prepared B / N co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0065] Example 10
[0066] The difference between Example 10 and Example 3 is that the manganese to iron ratio of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the primary positive electrode active material in this example includes the following steps:
[0067] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.7:0.3:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.7 Fe 0.3 PO4.
[0068] Embodiment 11
[0069] The difference between Example 11 and Example 3 is that the manganese to iron ratio of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the primary positive electrode active material in this example includes the following steps:
[0070] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.5:0.5:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.5 Fe 0.5 PO4.
[0071] Example 12
[0072] The difference between Example 12 and Example 3 is that the manganese to iron ratio of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the primary positive electrode active material in this example includes the following steps:
[0073] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.9:0.1:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.9 Fe 0.1 PO4.
[0074] Example 13
[0075] The difference between Example 13 and Example 3 is that the manganese to iron ratio of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the primary positive electrode active material in this example includes the following steps:
[0076] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.8:0.2:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.8 Fe 0.2 PO4.
[0077] Embodiment 14
[0078] The difference between Example 14 and Example 3 is that the content of the carbon layer coated on the surface of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the positive electrode material described in this example includes the following steps:
[0079] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0080] S2. The primary positive electrode active material, glucose and sublimed sulfur were weighed in a mass ratio of 85:10:5, a small amount of deionized water was added, high-energy ball milling was performed for 6 hours, drying was performed, and then sintering was performed at 550°C for 4 hours in an ammonia-argon mixed atmosphere (the volume fraction of ammonia was 5%) to obtain S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 2wt%.
[0081] S3. Prepared S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0082] Embodiment 15
[0083] The difference between Example 15 and Example 3 is that the content of the carbon layer coated on the surface of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the positive electrode material described in this example includes the following steps:
[0084] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0085] S2. The primary positive electrode active material, glucose and sublimed sulfur were weighed in a mass ratio of 75:20:5, a small amount of deionized water was added, high-energy ball milling was performed for 6 hours, drying was performed, and then sintering was performed at 550°C for 4 hours in an ammonia-argon mixed atmosphere (the volume fraction of ammonia was 5%) to obtain S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 4wt%.
[0086] S3. Prepared S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0087] Example 16
[0088] The difference between Example 16 and Example 3 is that the content of the carbon layer coated on the surface of lithium manganese iron phosphate in the positive electrode material is different. The preparation method of the positive electrode material described in this example includes the following steps:
[0089] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0090] S2. The primary positive electrode active material, glucose and sublimed sulfur were weighed in a mass ratio of 90:5:5, a small amount of deionized water was added, high-energy ball milling was performed for 6 hours, drying was performed, and then sintering was performed at 550°C for 4 hours in an ammonia-argon mixed atmosphere (the volume fraction of ammonia was 5%) to obtain S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 1wt%.
[0091] S3. Prepared S / N co-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0092] Embodiment 17
[0093] The difference between Example 17 and Example 3 is that the carbon coating layer on the surface of lithium manganese iron phosphate in the positive electrode material is doped with different elements. The preparation method of the positive electrode material in Example 17 includes the following steps:
[0094] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0095] S2. Weigh the primary positive electrode active material and glucose in a mass ratio of 85:15, add a small amount of deionized water, high-energy ball mill for 6 hours, dry, and then sinter at 550°C for 4 hours in an ammonia-argon mixed atmosphere (ammonia volume fraction of 5%) to obtain N-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 3wt%.
[0096] S3. Prepared N-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0097] Embodiment 18
[0098] The difference between Example 18 and Example 3 is that the carbon coating layer on the surface of lithium manganese iron phosphate in the positive electrode material is doped with different elements. The preparation method of the positive electrode material in Example 18 includes the following steps:
[0099] S1. Lithium carbonate, manganese sulfate, ferrous sulfate and ammonium dihydrogen phosphate were added into a ball mill according to a molar ratio of 0.5:0.6:0.4:1, and then ball milled for 24 hours. The precursor obtained by ball milling was placed in a tube furnace for calcination. The temperature was first increased to 350°C at a heating rate of 3°C / min for pre-calcination for 240 minutes, and then increased to 700°C at a heating rate of 5°C / min, calcined for 640 minutes, and the primary positive electrode active material was obtained after natural cooling. The primary positive electrode active material is LiMn 0.6 Fe 0.4 PO4;
[0100] S2. The primary positive electrode active material, glucose and sublimed sulfur were weighed in a mass ratio of 80:15:5, and a small amount of deionized water was added. The mixture was subjected to high-energy ball milling for 6 hours, dried, and then sintered at 550°C for 4 hours in an argon atmosphere to obtain S-doped carbon-coated LiMn 0.6 Fe 0.4 PO4 materials, including LiMn 0.6 Fe 0.4 The weight percentage of the carbon layer coated on the surface of the PO4 material is 3wt%.
[0101] S3. Prepared S-doped carbon-coated LiMn 0.6 Fe 0.4 The PO4 material and lithium manganate are mixed in a weight ratio of 7:3 to obtain a positive electrode material.
[0102] Comparative Example 1
[0103] The difference between Comparative Example 1 and Example 3 is that the positive electrode active material only contains lithium iron manganese oxide and does not contain lithium manganese oxide.
[0104] The physical properties of the positive electrode materials in Examples 1 to 18 and Comparative Example 1 are shown in Table 1.
[0105] SOC-OCV offset test method:
[0106] The secondary batteries prepared in Examples 1 to 18 and Comparative Example 1 were subjected to SOC-OCV testing using a charge and discharge testing system. The testing steps are as follows:
[0107] 1. Adjust the temperature to 25℃ and let it stand for 120 minutes;
[0108] 2.1 / 3C DC to 2.5V, let stand for 30min;
[0109] 3.1 / 3C CC to 4.25V and CV to 0.05C, let stand for 30min;
[0110] 4.1 / 3C DC to 2.5V, let stand for 30min;
[0111] 5. Repeat steps 3 to 4 three times, and take the third release capacity as Q0;
[0112] 6.1 / 3C CC to 4.25V and CV to 0.05C, rest 180min, record voltage;
[0113] 7. Adjust the temperature to 25°C, let stand for 120 minutes, release 5% Q0 at 1 / 3C (adjust to 95% SOC), let stand for 180 minutes, and record the voltage;
[0114] 8. Adjust the temperature to 25°C, let stand for 120 minutes, release 5% Q0 at 1 / 3C (adjust to 90% SOC), let stand for 180 minutes, and record the voltage;
[0115] 9. Adjust the temperature to 25°C, let stand for 120 minutes, release 5% Q0 at 1 / 3C (adjust to 85% SOC), let stand for 180 minutes, and record the voltage;
[0116] 10. Adjust the temperature to 25°C, let stand for 120 minutes, release 5% Q0 at 1 / 3C (adjust to 80% SOC), let stand for 180 minutes, and record the voltage;
[0117] 11. Repeat step 10, adjust the SOC to 75% / 70% / 65%...10% / 5% (every 5% SOC) in sequence, and record the voltage after standing at 25°C for 180 minutes;
[0118] 12. Adjust the temperature to 25°C, let stand for 120 min, release 2.5% Q0 at 0.1C (adjust to 2.5% SOC), let stand for 180 min, and record the voltage;
[0119] 13. Adjust the temperature to 25°C, let stand for 120 min, release 2% Q0 at 0.1C (adjust to 0.5% SOC), let stand for 180 min, and record the voltage;
[0120] 14. Adjust the temperature to 25℃, let it stand for 120min, discharge 0.5% Q0 at 0.1C (note that the lower limit of the discharge protection voltage in this step is 2.5V), let it stand for 180min, and record the voltage;
[0121] Note: DC stands for constant current discharge, CC stands for constant current charge, and CV stands for constant voltage charge.
[0122] The SOC-OCV curves before and after the battery cycle were tested. The OCV offset was obtained by subtracting the voltages at the same SOC. The results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] It can be seen from the above embodiments and comparative examples that by mixing lithium manganese oxide into lithium iron manganese oxide and doping specific inorganic non-metallic elements into the carbon coating layer of lithium iron manganese oxide, the problem of serious deviation of the SOC-OCV curve of the lithium iron manganese oxide secondary battery throughout its life cycle can be improved.
[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A positive electrode material, characterized in that: The positive electrode material includes manganese iron lithium oxide and lithium manganate, at least part of the surface of the manganese iron lithium oxide has a carbon coating layer, the carbon coating layer contains inorganic non-metallic elements, and the inorganic non-metallic elements include non-metallic elements in group IIIA, VA or VIA.
2. The positive electrode material according to claim 1, characterized in that The inorganic non-metallic element includes at least one of S, N, P and B.
3. The positive electrode material according to claim 1, characterized in that Based on the total weight of the manganese iron lithium oxide, the content of the carbon coating layer is 1 wt % to 4 wt %.
4. The positive electrode material according to claim 1, characterized in that The weight percentage of lithium manganese oxide in the positive electrode material is n1wt%, satisfying: n1≥10.
5. The positive electrode material according to claim 4, characterized in that Satisfies: n1≥30.
6. The positive electrode material according to claim 1, characterized in that The molar ratio of manganese atoms to iron atoms in the manganese-iron lithium oxide is Mn / Fe≥1.
7. The positive electrode material according to claim 6, characterized in that The molar ratio of manganese atoms to iron atoms in the manganese-iron lithium oxide is 7:3 to 9:
1.
8. A secondary battery, characterized in that: It comprises a positive electrode plate, wherein the positive electrode plate comprises the positive electrode material according to any one of claims 1 to 7.
9. The secondary battery according to claim 8, characterized in that: The compaction density of the positive electrode sheet is 2.36-3.05 g / cm 3 .
10. An electrical device, characterized in that: The electrical device comprises the secondary battery according to claim 8 or 9.
Citation Information
Cited By
Lithium ion battery, positive electrode active material and preparation method therefor, and electric device
WO2026179414A1