Coating liquid, positive pole piece and lithium battery thereof

By using a coating solution modified by sulfonic acid-based metal organic framework particles in the positive electrode sheet of the lithium battery, the problem of insufficient adsorption capacity of impurities in existing lithium batteries is solved, and the safety and service life of the lithium battery is significantly improved, so as to achieve Higher cycle performance and capacity retention.

CN118970045APending Publication Date: 2024-11-15ANHUI LIKE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411015728.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium battery positive electrode plate cannot effectively improve the circulation performance and service life of lithium batteries, and cannot remove impurities and ions in the lithium battery system, affecting the safety and life of the battery.

Method used

Using a coating liquid, including bio-based particles, sulfonic acid-based metal organic framework particles, positive electrode active materials, conductive agents and binders, the metal organic framework particles are modified by sulfonic acid groups to enhance their tolerance to nickel, cobalt, and manganese. The adsorption ability of plasma avoids the precipitation of positive electrode materials and improves battery safety and life.

Benefits of technology

The positive electrode sheet prepared by the coating solution can effectively adsorb impurity ions, reduce battery short circuits, improve the safety and service life of lithium batteries, and significantly improve cycle performance and capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970045A_ABST
    Figure CN118970045A_ABST
Patent Text Reader

Abstract

The invention discloses a coating liquid, a positive pole piece and a lithium battery thereof. The coating liquid comprises the following components in parts by mass: 1.0-3.0 parts of bio-based particles; 1-8 parts by mass of sulfonic metal organic framework particles; 90-96 parts by mass of a positive electrode active material; 0.5 to 1.6 parts by mass of a conductive agent; 1-2 parts by mass of a binder; 5-7 parts by mass of water; the preparation method of the sulfonic acid-based metal organic framework particles comprises the following steps: dissolving metal ions and a carboxyl-containing compound in a solvent for a first reaction to form a mixed solution, and then filtering, washing and drying to obtain metal organic framework particles; and mixing the metal organic framework particles with dichloromethane and chlorosulfonic acid, and carrying out a second reaction to obtain the sulfonic acid-based metal organic framework particles. The positive pole piece prepared from the coating liquid can absorb and adsorb ions such as nickel, cobalt and manganese in the battery, and separation of a positive pole material is avoided, so that the safety of the battery is improved, and the service life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a coating liquid, a positive electrode sheet and a lithium battery thereof. Background Art

[0002] With the gradual consumption of global energy, available non-renewable energy will become less and less, and the use of non-renewable energy will bring challenges to the environment, such as global warming, haze, etc. Therefore, many countries are vigorously developing sustainable energy.

[0003] Lithium batteries have attracted much attention in sustainable energy due to their advantages such as sustainable use, good for the environment, safety and convenience. Lithium batteries are generally composed of positive electrodes, negative electrodes, separators and electrolytes. The performance of the positive electrode plays a crucial role in the performance of lithium batteries.

[0004] The positive electrode sheet of the existing lithium battery is usually made by attaching a certain proportion of positive active material and conductive agent to the positive current collector through a binder and using a certain process to make the electrode. However, the lithium battery made of the existing positive electrode sheet cannot effectively improve the cycle performance of the lithium battery and cannot remove the impurity ions in the lithium battery system, thus affecting the cycle performance and service life of the lithium battery.

[0005] Therefore, the performance of existing positive electrode plates needs to be improved. Summary of the invention

[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a coating liquid, a positive electrode plate and a lithium battery thereof, wherein the positive electrode plate prepared by the coating liquid can absorb and adsorb nickel, cobalt, manganese and other ions in the battery to avoid the precipitation of positive electrode materials, thereby improving the safety and service life of the battery.

[0007] In one aspect of the present invention, the present invention provides a coating liquid. According to an embodiment of the present invention, the coating liquid comprises:

[0008] 1.0 to 3.0 parts by mass of bio-based particles;

[0009] 1 to 8 parts by weight of sulfonic acid metal organic framework particles;

[0010] 90 to 96 parts by weight of positive electrode active material;

[0011] 0.5 to 1.6 parts by mass of a conductive agent;

[0012] 1 to 2 parts by mass of a binder;

[0013] 5-7 parts by weight of water;

[0014] The preparation method of the sulfonic acid metal organic framework particles comprises: dissolving metal ions and carboxyl compounds in a solvent for a first reaction to form a mixed solution, then filtering, washing and drying to obtain metal organic framework particles; and then mixing the metal organic framework particles with dichloromethane and chlorosulfonic acid for a second reaction to obtain sulfonic acid metal organic framework particles.

[0015] According to the coating liquid of the embodiment of the present invention, by introducing the sulfonic acid group -SO3H into the metal organic framework particles, the sulfonic acid metal organic framework particles are obtained. The metal organic framework particles are porous, and the solution can enter their pores. The introduction of the sulfonic acid group can modify their pores, which is conducive to the metal organic framework particles to better adsorb impurity ions and reduce battery short circuits. At the same time, the sulfonic acid group can absorb and adsorb nickel, cobalt, manganese and other ions in the battery to avoid the precipitation of the positive electrode material, thereby improving the safety and service life of the battery.

[0016] In addition, the coating liquid according to the above embodiment of the present invention may also have the following additional technical features:

[0017] In some embodiments of the present invention, the metal ions are one or more of copper, iron, zinc, aluminum, cobalt, iron, nickel and magnesium.

[0018] In some embodiments of the present invention, the carboxyl-containing compound is one or more of terephthalic acid, trimesic acid, 2-hydroxyterephthalic acid and 2-aminoterephthalic acid.

[0019] In some embodiments of the present invention, the solvent is one or more of N-methylpyrrolidone, 1,5-dimethyl-2-pyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

[0020] In some embodiments of the present invention, the mass ratio of the metal ion to the carboxyl-containing compound is 1:(0.5-3.5), and the ratio of the carboxyl-containing compound to the solvent is (1-20) mg:1 mL.

[0021] In some embodiments of the present invention, the ratio of the metal organic framework particles, chlorosulfonic acid and dichloromethane is 1 g: (0.3-0.6) g: (25-50) mL.

[0022] In some embodiments of the present invention, the temperature of the first reaction is 90-220°C, and the reaction time is 10-100 hours; the time of the second reaction is 0.5-3 hours, and the temperature is -2-2°C.

[0023] In some embodiments of the present invention, the bio-based particles are one or more of furan-based polyamide, furan-based polyimide and furan polyester, with a particle size of 0.01 to 0.1 μm and a thermal decomposition temperature of >400°C.

[0024] In some embodiments of the present invention, the positive electrode active material is one or more of lithium cobalt oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium manganese oxide; the conductive agent is at least one of carbon black, conductive graphite, graphene and carbon nanotubes; and the binder is one or more of polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile, polyimide and polyurethane.

[0025] In the second aspect of the present invention, the present invention proposes a positive electrode plate. According to an embodiment of the present invention, the positive electrode plate includes: a positive electrode current collector; a coating, wherein the coating is formed by coating the above-mentioned coating liquid on at least one side of the positive electrode current collector, and the thickness of the coating is 1 to 4 μm. As a result, the positive electrode plate can better adsorb impurity ions and reduce battery short circuits. At the same time, it can absorb and adsorb nickel, cobalt, manganese and other ions in the battery to avoid the precipitation of positive electrode materials, thereby improving the safety and service life of the battery.

[0026] In a third aspect of the present invention, the present invention provides a lithium-ion battery. According to an embodiment of the present invention, the lithium-ion battery comprises the above-mentioned positive electrode sheet. Thus, the safety and service life of the lithium-ion battery are improved.

[0027] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0029] Figure 1 This is a cycle curve diagram of the lithium battery prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0030] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0031] Example 1

[0032] Preparation of positive electrode coating liquid: Mix 1.1 parts by mass of furan-based polyamide particles, 2 parts by mass of sulfonic acid metal organic framework particles, 91 parts by mass of lithium cobalt oxide, 0.8 parts by mass of carbon black, 1.1 parts by mass of polyvinylidene fluoride and 5.1 parts by mass of water, stir evenly, and make a positive electrode coating liquid.

[0033] The preparation method of sulfonic acid metal organic framework particles includes: dissolving 5g of copper nitrate and 3g of terephthalic acid in 500mL of N,N-dimethylformamide, reacting for 90h at a reaction temperature of 200°C to obtain a mixed solution, then filtering the mixed solution, washing it with ethanol, and vacuum drying it for 10h to finally obtain solid Cu@MOF particles, which are ground for standby use. Then, 1g of Cu@MOF particles is mixed with 26mL of dichloromethane and 0.4g of chlorosulfonic acid, reacting at 0°C for 1h, and then filtering and washing to obtain sulfonic acid metal organic framework particles.

[0034] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0035] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0036] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0037] Example 2

[0038] Preparation of positive electrode coating liquid: Mix 1.1 parts by mass of furan-based polyimide particles, 2 parts by mass of sulfonic acid metal organic framework particles, 91 parts by mass of lithium iron phosphate, 0.8 parts by mass of conductive graphite, 1.1 parts by mass of polyvinylidene fluoride and 5.1 parts by mass of water, stir evenly, and make a positive electrode coating liquid.

[0039] The preparation method of sulfonic acid metal organic framework particles includes: dissolving 5g of copper nitrate and 3g of terephthalic acid in 500mL of N,N-dimethylformamide, reacting for 90h at a reaction temperature of 200°C to obtain a mixed solution, then filtering the mixed solution, washing it with ethanol, and vacuum drying it for 10h to finally obtain solid Cu@MOF particles, which are ground for standby use. Then, 1g of Ni@MOF particles is mixed with 26mL of dichloromethane and 0.4g of chlorosulfonic acid, reacting at 0°C for 1h, and then filtering and washing to obtain sulfonic acid metal organic framework particles.

[0040] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0041] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0042] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0043] Example 3

[0044] Preparation of positive electrode coating liquid: Mix 2.8 parts by mass of furan-based polyamide particles, 7.5 parts by mass of sulfonic acid metal organic framework particles, 95 parts by mass of lithium cobalt oxide, 1.5 parts by mass of carbon black, 1.9 parts by mass of polyvinylidene fluoride and 7.8 parts by mass of water, stir evenly, and make a positive electrode coating liquid.

[0045] The preparation method of sulfonic acid metal organic framework particles includes: dissolving 5g of magnesium nitrate and 3g of trimesic acid in 500mL of 1,5-dimethyl-2-pyrrolidone, reacting for 60h at a reaction temperature of 100°C to obtain a mixed solution, then filtering the mixed solution, washing it with ethanol, and vacuum drying it for 10h to finally obtain solid Mg@MOF particles, which are ground for standby use. Then, 1g of Mg@MOF particles is mixed with 26mL of dichloromethane and 0.4g of chlorosulfonic acid, reacting at 0°C for 1h, and then filtering and washing to obtain sulfonic acid metal organic framework particles.

[0046] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0047] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0048] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0049] Example 4

[0050] Preparation of positive electrode coating liquid: Mix 1.1 parts by mass of furan-based polyamide particles, 2 parts by mass of sulfonic acid metal organic framework particles, 91 parts by mass of lithium cobalt oxide, 0.8 parts by mass of carbon black, 1.1 parts by mass of polyvinylidene fluoride and 5.1 parts by mass of water, stir evenly, and make a positive electrode coating liquid.

[0051] The preparation method of sulfonic acid metal organic framework particles includes: dissolving 5g of copper nitrate and 3g of terephthalic acid in 500mL of N,N-dimethylformamide, reacting for 90h at a reaction temperature of 200°C to obtain a mixed solution, then filtering the mixed solution, washing it with ethanol, and vacuum drying it for 10h to finally obtain solid Cu@MOF particles, which are ground for standby use. Then, 1g of Cu@MOF particles is mixed with 26mL of dichloromethane and 0.4g of chlorosulfonic acid, reacting at 0°C for 1h, and then filtering and washing to obtain sulfonic acid metal organic framework particles.

[0052] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0053] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0054] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0055] Comparative Example 1

[0056] No sulfonic acid metal organic framework particles were added, and the rest of the process was the same as in Example 1 to prepare a coating liquid.

[0057] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0058] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0059] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0060] Comparative Example 2

[0061] Without adding bio-based particles, the remaining process was the same as in Example 1 to prepare a coating liquid.

[0062] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0063] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0064] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0065] Comparative Example 3

[0066] Without adding sulfonic acid metal organic framework particles and bio-based particles, the remaining process was the same as in Example 1 to prepare a coating liquid.

[0067] Preparation of positive electrode sheet: The positive electrode sheet coating liquid is coated on one side of the positive electrode current collector aluminum foil, the coating thickness is 3 μm, and then dried to obtain the negative electrode sheet.

[0068] Battery assembly: Assemble a lithium battery using the prepared positive electrode sheet as the positive electrode, graphite as the negative electrode, glass fiber as the separator, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate (EC) and diethyl carbonate (EMC) as the electrolyte.

[0069] The assembled battery was subjected to electrochemical testing: charge and discharge cycles were performed at a 1C rate (1C is calculated as 1000mAh / g), the voltage range was 0-1.5V, the number of cycles was 100, and the rate performance test was performed at a 2C rate. The negative electrode sheet was disassembled from the battery after 100 cycles, and the expansion rate of the negative electrode sheet was measured. The relevant test results are shown in Table 1.

[0070] Table 1 Cyclic performance results of lithium batteries prepared in Examples 1-4 and Comparative Examples 1-3

[0071]

[0072] From the data in Table 1, it can be seen that the capacity retention rate of the lithium batteries prepared in Examples 1-4 is still above 95% after 100 cycles at 1C. Figure 1 It can be seen from the cyclic voltammetry curve of the lithium battery obtained in Example 2 that the capacity retention rate is still about 98% after 120 cycles.

[0073] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0074] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A coating liquid, characterized in that: include: 1 to 3 parts by weight of bio-based particles; 1 to 8 parts by weight of sulfonic acid metal organic framework particles; 90-96 parts by weight of positive electrode active material; 0.5 to 1.6 parts by mass of a conductive agent; 1 to 2 parts by mass of a binder; 5 to 7 parts by weight of water; The preparation method of the sulfonate metal organic framework particles comprises: dissolving metal ions and carboxyl compounds in a solvent for a first reaction to form a mixed solution, and then filtering, washing and drying to obtain metal organic framework particles; and then mixing the metal organic framework particles with dichloromethane and chlorosulfonic acid for a second reaction to obtain sulfonate metal organic framework particles.

2. The coating liquid according to claim 1, characterized in that: The metal ions are one or more of copper, iron, zinc, aluminum, cobalt, iron, nickel and magnesium; The carboxyl-containing compound is one or more of terephthalic acid, trimesic acid, 2-hydroxyterephthalic acid and 2-aminoterephthalic acid; The solvent is one or more of N-methylpyrrolidone, 1,5-dimethyl-2-pyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

3. The coating liquid according to claim 1, characterized in that: The mass ratio of the metal ion to the carboxyl-containing compound is 1:(0.5-3.5), and the ratio of the carboxyl-containing compound to the solvent is (1-20) mg:1 mL.

4. The coating liquid according to claim 1, characterized in that: The ratio of the metal organic framework particles, chlorosulfonic acid and dichloromethane is 1 g: (0.3-0.6) g: (25-50) mL.

5. The coating liquid according to claim 1, characterized in that: The temperature of the first reaction is 90 to 220° C., and the reaction time is 10 to 100 hours; the time of the second reaction is 0.5 to 3 hours, and the temperature is -2 to 2° C.

6. The coating liquid according to claim 1, characterized in that: The bio-based particles are one or more of furan-based polyamide, furan-based polyimide and furan polyester, with a particle size of 0.01 to 0.1 μm and a thermal decomposition temperature of more than 400° C.

7. The coating liquid according to claim 1, characterized in that: The positive electrode active material is one or more of lithium cobalt oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium manganese oxide; the conductive agent is at least one of carbon black, conductive graphite, graphene and carbon nanotubes; the binder is one or more of polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile, polyimide and polyurethane.

8. A positive electrode sheet, characterized in that: include: Positive electrode current collector; A coating layer, wherein the coating layer is formed by coating the coating liquid according to any one of claims 1 to 7 on at least one side of the positive electrode current collector, and the thickness of the coating layer is 1 to 4 μm.

9. A lithium battery, characterized in that: Including the positive electrode sheet as described in claim 8.

Citation Information

Cited By

  • Preparation method of high-performance biomass-based hard carbon negative electrode material

    CN119601586A