Lithium ion battery
By using modified components in lithium-ion batteries and hydrogenated nitrile rubber, the stability and electrolyte compatibility of HNBR in extreme environments is solved, the performance and life of the battery are improved, and the charging is achieved Discharge efficiency and cycle stability.
Patent Information
- Application Number
- CN202411443103.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The service life and stability of hydrogenated nitrile rubber (HNBR) in lithium-ion batteries are affected by extreme environment, and compatibility issues with electrolytes lead to degradation of battery performance, and there are few related research.
Hydrogenated nitrile rubber is used as the positive electrode binder, and the modified components such as lithium difluorosulfonylimide, lithium dioxalic acid borate, and fluorovinyl carbonate are mixed to form a high-quality positive electrode slurry to improve the electrode material. Stability and battery performance.
Effectively isolate active substances and HNBR, improve battery charge and discharge efficiency and cycle stability, extend service life, reduce side reactions, and promote the upgrading of lithium-ion battery technology.
Smart Images

Figure CN118970055A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy battery materials, and in particular relates to a lithium-ion battery. Background Art
[0002] With the rapid development of the new energy vehicle industry, lithium-ion batteries have been widely used in our lives. In lithium-ion batteries, battery binders are an important component of lithium-ion batteries. Although the weight percentage of binders in electrode materials is low, it can seriously affect the electrochemical properties of electrodes. Binders with excellent performance and appropriate dosage can allow batteries to obtain larger capacity, longer cycle life and lower internal resistance, which promotes improving the battery's cycle performance, fast charging and discharging capabilities, and reducing the internal pressure of the battery. Binders are important components of conductive slurries and electrodes, and play a role in dispersing / bonding active substances and conductive agents. If the binder is unevenly dissolved or forms agglomerates in the electrode slurry composition, it will affect the coating performance of the electrode slurry. At present, polyvinylidene fluoride (PVDF) is the most important binder used in the positive electrode of lithium-ion batteries.
[0003] However, as the use of fluorine-containing materials becomes increasingly strict, hydrogenated nitrile rubber (HNBR) has become a key candidate material to replace PVDF. After using HNBR as a binder or dispersant, the electrolyte will penetrate into the electrode more easily, while ensuring the excellent conductivity of the conductive agent, reducing the electrode resistance, and improving the cycle performance of the battery. At the same time, HNBR also has excellent bonding properties and electrochemical stability, and does not contain fluorine, which is more environmentally friendly and safe in production and use processes. However, compared with PVDF, HNBR also has the following two problems: ① Service life and stability: The life and stability of HNBR depend on the use conditions and environmental factors. If the battery is often in extreme temperature, humidity or chemical environment, the HNBR binder may age or degrade faster; ② The problem of electrolyte compatibility; HNBR may interact with some components in the electrolyte, which may cause the electrolyte to fail, thereby reducing the performance and service life of the battery; Among them, ① involves the use environment, which will have an important impact on the performance of HNBR (life, stability, charge and discharge efficiency, rate performance, etc.). Therefore, in order to meet the performance requirements of lithium-ion batteries for binders, it is necessary to provide an HNBR binder with excellent comprehensive performance and use environment. Therefore, how to improve the use environment of HNBR in lithium-ion batteries and how to optimize the interface reaction between HNBR and active substances are still a difficult problem that needs to be solved and optimized urgently. There are few related studies or no substantial reports on related experiments. Summary of the invention
[0004] The invention provides a lithium ion battery using HNBR as a positive electrode binder to improve battery performance.
[0005] In order to achieve the above object, the present invention is implemented by the following technical solutions:
[0006] A lithium-ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte; the positive electrode adopts hydrogenated nitrile rubber (HNBR) as a binder, and is obtained by mixing a positive electrode active material, hydrogenated nitrile rubber, a conductive agent and a solvent to form a positive electrode slurry, and evenly coating the positive electrode slurry on a current collector and then drying the mixture;
[0007] The hydrogen saturation of the hydrogenated nitrile rubber is ≥90%; the acrylonitrile (ACN) content is 16%-50%; the Mooney viscosity ML (1+4) @ 100°C is 20-85 or the molecular weight Mw is 20000-40000;
[0008] The positive electrode slurry or electrolyte further contains a modified component, and the modified component is selected from one or more of lithium bis(fluorosulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiDFOB), fluoroethylene carbonate, lithium bis(oxalatoborate), and trifluoroethylphosphite.
[0009] Preferably, the hydrogen saturation of the hydrogenated nitrile rubber is ≥95%, and the more preferred hydrogenation saturation is >99%.
[0010] Preferably, the acrylonitrile (ACN) content of the hydrogenated nitrile rubber is 22%-40%, more preferably 26%-34%, and even more preferably 26%-29%.
[0011] Preferably, the Mooney viscosity ML(1+4)@100°C of the hydrogenated nitrile rubber is 20-75, more preferably 20-70, such as 20-30.
[0012] Preferably, the molecular weight Mw of the hydrogenated nitrile rubber is 30,000-40,000.
[0013] According to the above scheme, the positive electrode active material is lithium iron phosphate (LFP), lithium manganese phosphate, lithium cobalt phosphate, lithium manganese iron phosphate, lithium nickel iron phosphate, lithium manganese cobalt phosphate, lithium cobalt oxide (LCO), lithium cobalt manganese oxide, lithium nickel cobalt manganese oxide (Li 10 Ni x Co y Mn z O 20 , referred to as NCMxyz, xyz is the molar ratio of nickel, cobalt and manganese (x=2-8, y=1-5, z=1-5, satisfying x+y+z=10), preferably lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide (NCM523), or lithium cobalt manganese oxide, more preferably LFP, LCO or NCM523.
[0014] According to the above scheme, the conductive agent is one or more of conductive carbon black, Ketjen black, carbon fiber, carbon nanotube, and graphene, preferably conductive carbon black, carbon fiber or carbon nanotube, and more preferably conductive carbon black.
[0015] According to the above scheme, the solvent of the positive electrode slurry is one or more of N-methyl-2-pyrrolidone (NMP), acetone, ethylene glycol dimethyl ether, and anisole, preferably NMP, ethylene glycol dimethyl ether or anisole, and more preferably NMP.
[0016] According to the above scheme, taking the total mass of the positive electrode active material, hydrogenated nitrile rubber and conductive agent as 100%, the mass percentages of the positive electrode active material, hydrogenated nitrile rubber and conductive agent are 80-92 wt%, 4-10 wt% and 4-10 wt% respectively.
[0017] According to the above solution, the separator of the lithium-ion battery is one of a polyethylene microporous membrane, a glass fiber membrane or a polypropylene microporous membrane, preferably a polypropylene microporous membrane Celgard2400.
[0018] According to the above scheme, the electrolyte includes a lithium salt and a solvent, and the solvent is one or more of propylene carbonate, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate, and polyethylene oxide, preferably a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC), and more preferably EC:EMC:DMC=1:1:1 (volume ratio).
[0019] The lithium salt is one or more of LiFP6, LiBF4, LiAsF4, LiClO4, LiFSI, and LiNO3, preferably LiFP6, LiBF4 or LiNO3, and more preferably LiFP6.
[0020] According to the above scheme, the lithium salt concentration in the electrolyte is 0.3-3.0 M, preferably 0.5-2.0 M, and more preferably 0.8-1.5 M.
[0021] According to the above scheme, the modifying component is LiTFSI and / or LiDFOB.
[0022] According to the above scheme, the positive electrode slurry contains a modified component, and the modified component is added by way a or way b:
[0023] Method a: Under the protection of inert gas, HNBR and modified components are dispersed in a solvent and fully dispersed (preferably magnetically stirred at room temperature for 4-8 h) to obtain a binder solution, and then the lithium salt, binder solution and conductive agent are mixed evenly to obtain a positive electrode slurry; preferably, the mass ratio of HNBR to the modified component is 1:0.5-2.0, more preferably 1:1.
[0024] Mode b: Under the protection of inert gas, the positive electrode active material, hydrogenated nitrile rubber, conductive agent and modified component are directly mixed in a solvent and fully dispersed (preferably magnetically stirred at room temperature for 4-6 hours) to obtain a positive electrode slurry; preferably, the mass ratio of HNBR to the modified component is 1:0.5-2.0, more preferably 1:1.
[0025] According to the above scheme, the electrolyte also contains a modifying component, and the content of the modifying component is 0.5-2.0% of the amount of lithium salt used, preferably 1.0%.
[0026] According to the above solution, the current collector is a metal foil or a metal mesh structure, preferably a metal foil, and more preferably an aluminum foil treated with carbon coating.
[0027] According to the above scheme, the negative electrode is any one or more of metal lithium sheet, lithium alloy, graphite, silicon, silicon oxide, silicon alloy, tin, and tin alloy, preferably metal lithium sheet and graphite.
[0028] According to the above scheme, the separator is a glass fiber membrane, a polyethylene microporous membrane, a polypropylene microporous membrane or an ethylene-propylene copolymer microporous membrane, preferably a polypropylene microporous membrane.
[0029] According to the above solution, the lithium ion battery is a liquid lithium ion battery.
[0030] According to the above scheme, the lithium-ion battery can be assembled into a button battery, a soft-pack battery or a cylindrical battery.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] ① This method effectively isolates the active material and HNBR by forming a high-quality film on the surface of the active material. It has low requirements on the HNBR model and positive electrode material and has wide applicability.
[0033] ② This method belongs to the in-situ modification in the battery, and does not involve traditional modification methods such as nano-, composite, and doping of positive electrode materials. It has the advantages of strong practicality, easy promotion, and low cost;
[0034] ③This scheme can not only maintain the binding force between electrode components and between electrode and current collector, but also greatly enhance the stability of the structure and properties of battery active materials and HNBR in the charging and discharging environment, thereby effectively improving the battery's charging and discharging efficiency, cycle stability and service life, while reducing the side reactions of the battery under operating conditions, which is of great value to promoting the technological upgrading of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The effects of different modified components on the performance of sample 1-HNBR-LFP described in Example 1;
[0036] Figure 2 The effects of different modified components on the performance of sample 2-HNBR-LFP described in Example 2;
[0037] Figure 3 The effects of different modified components on the performance of sample 3-HNBR-LFP described in Example 3;
[0038] Figure 4 The effects of different modified components on the performance of the sample 1-HNBR-LCO electrode described in Example 4;
[0039] Figure 5 The effects of different modified components on the performance of sample 1-HNBR-NCM electrode described in Example 5;
[0040] Figure 6 The performance of different HNBR in LiDFOB / LiTFSI-LFP system described in Example 6;
[0041] Figure 7 The performance of different HNBR in LiDFOB / LiTFSI-LCO system described in Example 7;
[0042] Figure 8 The performance of different HNBRs in the LiDFOB / LiTFSI-NCM system described in Example 8. DETAILED DESCRIPTION
[0043] The present invention is described in detail below with reference to specific embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0044] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.
[0045] The preparation process of HNBR is as follows: under nitrogen replacement conditions, add some nitrile rubber and 500mL of anhydrous chlorobenzene to a 1L stainless steel reactor to make the mass concentration of the resulting solution 9%-13%. After complete dissolution under nitrogen sealing conditions, add "Jan's catalyst" (dosage is 0.08~0.13wt% of nitrile rubber), and heat to 60-100℃ (temperature 1) under nitrogen protection for degradation reaction for 0.5-2.0 hours (time 1), and the pressure is 1.0MPa. After adding hydrogen until the pressure reaches 8.0-8.5MPa (pressure 2), heat to 140~150℃ (temperature 2), react for 3-6 hours (time 2), and obtain a liquid HNBR solution. It is precipitated with methanol and vacuum dried at 110℃ to obtain HNBR. The ACN content in the obtained HNBR is consistent with the ACN content in the raw nitrile rubber, so different HNBR samples need to use nitrile rubber raw materials with corresponding ACN content. The specific preparation conditions of the HNBR sample used in the present invention are shown in Table 1.
[0046] Examples 1-8
[0047] Table 1 details the three key indicators of ACN content, hydrogen saturation and Mooney viscosity of samples 1-9 used in Examples 1-8. Among them, the ACN content is between 18% and 45%, the hydrogen saturation is 90%-99.9%, and the Mooney viscosity is between 20 and 85, covering the most representative HNBR types.
[0048] Table 1 Product parameters and preparation conditions of samples 1-9 used in Examples 1-8
[0049]
[0050] The sample characterization / battery performance test process described in Examples 1-8 includes three parts: pole piece preparation, battery assembly, and performance test. In order to ensure the rigor of the comparative analysis, in addition to the factors to be compared, Examples 1-8 adopted strict consistency in pole piece preparation, battery assembly, and performance test. The specific operation is as follows.
[0051] ① Preparation of pole piece: Take the positive electrode active material (LFP, LCO or NCM523), binder (PVDF or HNBR) and conductive carbon black in a ratio of 8:1:1 and mix and grind in an appropriate amount of NMP solvent (generally, the feed ratio of NMP to HNBR is 4mL:150mg. For a very small number of HNBRs that are difficult to dissolve, a little more NMP can be used, for example, 5mL:150mg, to ensure its dissolution) to obtain a uniform slurry. The slurry is evenly coated on aluminum foil with a coating thickness of 50 μm. After vacuum drying at 120°C for 12 hours, it is cut into pole pieces with a diameter of 12mm and placed in a glove box for use.
[0052] ②Battery assembly: The prepared positive electrode sheet is assembled into a liquid button battery in an argon-filled glove box (O2 and H2O contents are both <0.1ppm) in the order of negative electrode shell, spring gasket, stainless steel gasket, metallic lithium, diaphragm (polypropylene microporous membrane Celgard2400), electrolyte (1M LiFP6, EC:EMC:DMC=1:1:1 (volume ratio), modified components are one or two of LiDFOB and LiTFSI, and the content of modified components is 1.0% of LiFP6. When the modified components are LiTFSI+LiDFOB, the mass ratio of the two is 1:1), positive electrode sheet, and positive electrode shell.
[0053] ③ Performance test: The battery charging and discharging performance, coulomb efficiency and cycle performance were tested using Wuhan Blue Electric CT2001A battery testing system. Unless otherwise specified, all batteries of the present invention were tested at 25°C and 1C.
[0054] In the above steps ① to ③, the reagents, materials, dosages, preparation and testing conditions are only one of the most preferred schemes, but the embodiments of the present invention are not limited thereto.
[0055] Comparative Example
[0056] Preparation and testing: PVDF was assembled into batteries with LFP, LCO and NCM523 materials, and their cycling performances were studied with four different modified components (LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank control (no modified components added)). The specific preparation and testing processes are as described in steps ①-③ of Examples 1-8.
[0057] Performance description: Table 2 shows the performance of the battery described in this comparative example. By comparing the performance of the three positive electrode material-PVDF batteries with different modified components, the following conclusions can be drawn: The modified components have little effect on the three positive electrode material-PVDF batteries, and the changes in the four indicators of first-week capacity, first-week coulomb efficiency, first-week voltage difference, and long-cycle capacity retention rate are all within 1.5%.
[0058] Table 2 Performance of the battery described in the comparative example
[0059]
[0060] Figure 1 to Figure 8 The improvement effect and good applicability of the modified component on the HNBR binder are demonstrated from three aspects: modified component, active substance and HNBR type. Examples 1-8 will be described in detail in conjunction with the above charts.
[0061] Example 1
[0062] Preparation and testing: Assemble sample 1 and LFP material into a battery to study its cycling performance in four different modified components (LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank control (no modified component added)). The specific process is as described in steps ①-③ above. ① Preparation of pole piece: Take LFP, sample 1 and conductive carbon black in a mass ratio of 8:1:1, mix and grind in an appropriate amount of NMP solvent (generally, the feed ratio of NMP to HNBR is 4mL:150mg, and a little more NMP can be used for a very small number of HNBRs that are difficult to dissolve, such as 5 mL:150mg, to ensure its dissolution) to obtain a uniform slurry. The slurry is evenly coated on aluminum foil with a coating thickness of 50μm. After vacuum drying at 120℃ for 12 h, it is cut into pole pieces with a diameter of 12 mm and placed in a glove box for use. ②Battery assembly: The prepared positive electrode sheet was assembled into a liquid button cell in the order of negative electrode shell, spring gasket, stainless steel gasket, metal lithium, Celgard2400 diaphragm, electrolyte (1M LiFP6, EC:EMC:DMC=1:1:1 (volume ratio), the modified component was one of LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank control, and the content of the modified component was 1.0wt% of the amount of LiFP6 (when the modified component was LiTFSI+LiDFOB, the amount of the two was 0.5wt% of the amount of LiFP6, respectively), positive electrode sheet, and positive electrode shell in an argon-filled glove box (the content of O2 and H2O was <0.1ppm). ③Performance test: The charge and discharge performance, coulomb efficiency and cycle performance of the battery were tested using the Wuhan Blue Electric CT2001A battery test system, and the test conditions were 25°C and 1C rate.
[0063] Performance description: The battery performance of this embodiment is as follows Figure 1 As shown in the figure (500 cycles at 1C rate). It can be seen from the figure that LiTFSI+LiDFOB performs better in terms of initial capacity, reversible capacity, Coulombic efficiency, cycle stability, capacity retention rate, etc., followed by LiTFSI, then LiDFOB, and the blank group is the weakest; the reversible capacities in the first week are 140, 124, 109 and 118 mAh g -1 After 500 cycles, the reversible capacities are 128, 106, 75, and 21 mAh g -1 , the capacity retention rates were 91.4%, 85.5%, 68.8% and 17.8% respectively, with significant differences. This shows that the presence of the modified components affects the environment of the electrode reaction, especially the interface of the active material-electrolyte-binder. The electrolyte components determine the lithium ion migration speed, stability and film formation quality on the surface of the active material, all of which are directly related to the internal resistance and stability of the battery. The modified components make up for the obvious deficiencies of traditional electrolytes in these aspects, and have a significant effect on improving battery capacity and stability.
[0064] Example 2
[0065] Preparation and testing: The only difference from Example 1 is that the binder in the electrode preparation process is replaced by Sample 2 from Sample 1. The main difference between the two is the hydrogen saturation (96% for Sample 2 and >99% for Sample 1).
[0066] Performance comparison: The performance of all batteries in this example is as follows Figure 2 As shown. As can be seen from the figure, the performance of sample 2 in the four electrolytes is LiTFSI+LiDFOB>LiTFSI>LiDFOB>blank group. By comparing Examples 1 and 2, it can be found that the overall performance of sample 2 in the four electrolytes is weaker than that of sample 1, but when the modified component is present, its initial capacity, reversible capacity, coulombic efficiency, cycle stability, capacity retention rate and other aspects are better than the blank group. Among them, the performance of the LiTFSI+LiDFOB combination is the best.
[0067] Example 3
[0068] Preparation and testing: The only difference from Example 1 is that the binder in the electrode preparation process is replaced from Sample 1 to Sample 3. The main difference between the two is the hydrogen saturation. The hydrogen saturation of Sample 3 is 90%-92%, while that of Sample 1 is >99%.
[0069] Performance comparison: The performance of all batteries in this example is as follows Figure 3 As shown. As can be seen from the figure, the performance order of sample 3 in the four electrolytes is the same as that of sample 1 and sample 2, which is LiTFSI+LiDFOB>LiTFSI>LiDFOB>blank group. By comparing Examples 1-3, it can be found that the overall performance of sample 3 in the four electrolytes is weaker than that of sample 1 and sample 2, indicating that the lower hydrogen saturation is not conducive to the performance of the battery. However, in the presence of the modifying component, the initial capacity, reversible capacity, coulombic efficiency, cycle stability, capacity retention rate and other aspects of sample 3 are significantly better than those of the blank group. Among them, the performance of the LiTFSI+LiDFOB combination is the best.
[0070] Example 4
[0071] Preparation and testing: The only difference from Example 1 is that the active material in the electrode preparation process ① is replaced by LCO from LFP, and the effects of LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank group on the battery performance of sample 1-LCO are studied. Compared with LFP, LCO has a higher working potential and has higher oxidation resistance requirements for binders and electrolytes.
[0072] Performance comparison: The battery performance of this embodiment is as follows Figure 4As shown. In the presence of LiTFSI+LiDFOB, the initial capacity, reversible capacity, coulombic efficiency, cycle stability, capacity retention rate and other aspects of the sample 1-LCO battery are better; the reversible capacity of LiTFSI and LiDFOB is lower, but the stability is better; the blank group is the weakest and the capacity decay is the fastest. After 300 cycles, the capacity retention rate is only 44.9%. This shows that the presence of the modified component improves the reaction environment of sample 1-LCO. Among them, the performance of the LiTFSI+LiDFOB combination is the best.
[0073] Example 5
[0074] Preparation and testing: The only difference from Example 1 is that the active material in the electrode preparation process is replaced by NCM523 from LFP, and the effects of LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank group on the battery performance of sample 1-NCM523 are studied. Compared with LFP, the surface oxidation of NCM523 is higher and more susceptible to the electrochemical environment, so it puts forward higher requirements on the oxidation resistance of the binder and electrolyte.
[0075] Performance comparison: The battery performance of this embodiment is as follows Figure 5 As shown in the figure, LiTFSI+LiDFOB performs better in Coulombic efficiency and capacity retention, with a reversible capacity of 126 mAh g in the first week. -1 After 200 cycles, the capacity retention rate was 94.4%. The performance of LiTFSI was second, with a reversible capacity of 91 mAh g in the first cycle. -1 , good stability, after 200 cycles, the capacity remains at 100 mAh g -1 The LiDFOB and blank groups are the weakest, with initial capacities similar to those of LiTFSI, but poor cycle stability. This indicates that the LiTFSI+LiDFOB modified component has the best modification performance for the sample 1-NCM523 system.
[0076] Example 6
[0077] Preparation and testing: There are two differences from Example 1. First, the sample 1 in the preparation process of the pole piece is replaced with PVDF, sample 1 and samples 3 to 9, and the influence of different Mooney viscosity numbers (samples 1, 4, 5 and 8) and different ACN contents (samples 1, 6, 7 and 9) on the performance of LFP batteries is studied. Second, the modified component is replaced with LiTFSI+LiDFOB from four modified components, and the applicability of this component to different HNBR samples is studied.
[0078] Performance description: The battery performance of this embodiment is as follows Figure 6 As shown. ① The first-week reversible capacity of PVDF is 133 mAhg -1, the capacity retention rate after 500 cycles is 96.2%. Overall, when the LiTFSI+LiDFOB modified components exist, the long-cycle performance of the PVDF-LFP battery is good, but the initial reversible capacity is low. ② Samples 1, 4, 5 and 8 have different Mooney viscosities or molecular weights. Figure 6 It can be found that the Mooney viscosity number has a certain influence on the performance of HNBR in LFP. Among them, the reversible capacity and cycle stability of samples 1 and 8 are significantly better than those of PVDF. The initial capacity of sample 4 is much higher than that of PVDF, but the capacity decays faster, and the capacity after 500 weeks is comparable to that of PVDF. The initial capacity of sample 5 (130 mAh / g) is slightly lower than that of PVDF, but the cycle stability is significantly better, and the capacity remains at 128 mAh / g after 500 weeks. ③ The ACN contents of samples 1, 6, 7 and 9 are 26%~29%, 36.5%, 33% and 41%, respectively. The effect of HNBR binders with different ACN contents on LFP batteries is weak. The reversible capacity and cycle stability of samples 1, 6, 7 and 9 are significantly higher than those of PVDF. Combining this embodiment and embodiments 1-3, it can be concluded that in the LFP battery system, LiTFSI+LiDFOB has good applicability to various types of HNBR binders.
[0079] Example 7
[0080] Preparation and testing: The only difference from Example 6 is that the LFP in the electrode preparation process of ① is replaced with LCO. The applicability of the LiTFSI+LiDFOB combination to different HNBR samples in the LCO battery system is studied. Compared with LFP, LCO has a higher working potential and higher oxidation resistance requirements for the binder and electrolyte.
[0081] Performance description: The battery performance of this embodiment is as follows Figure 7 As shown. ① The first-week reversible capacity of PVDF is 137 mAhg -1, the capacity retention rate after 300 cycles is 95.6%. ② The Mooney viscosity number or molecular weight has a certain effect on the performance of HNBR in LCO (samples 1, 4, 5 and 8). Among them, the reversible capacity and cycle stability of sample 1 are significantly better than those of PVDF. Samples 4 and 8 are comparable to PVDF in reversible capacity or cycle stability. Sample 5 has the weakest performance, with a reversible capacity of 133mAh / g in the first week, slightly lower than PVDF. After 300 weeks, the capacity remains at 121mAh / g, with a retention rate of 91.6%. ③ HNBR binders with different ACN contents also have a certain effect on LCO batteries, but the effect is weak (samples 1, 6, 7 and 9). The reversible capacity and cycle stability of samples 6, 7 and 9 are comparable to those of PVDF. Among them, sample 6 has higher stability, and samples 7 and 9 have higher initial capacities. Combining ①-③, it can be concluded that in the LCO battery system, LiTFSI+LiDFOB has good applicability to various types of HNBR binders.
[0082] Example 8
[0083] Preparation and testing: The only difference from Example 6 is that the LFP in the electrode preparation process of ① is replaced with NCM523. The applicability of the LiTFSI+LiDFOB combination to different HNBR samples in the NCM523 battery system is studied. Compared with LFP and LCO, NCM523 has stronger surface oxidation ability and higher oxidation resistance requirements for binders and electrolytes.
[0084] Performance description: The battery performance of this embodiment is as follows Figure 8 ① The first-week reversible capacity of PVDF is 118 mAhg -1 , the capacity retention rate is 100% after 500 cycles, but there is a capacity climb in the first 20 weeks, which may be related to the large impedance of the interfacial film formed on the electrode surface. ② The effect of Mooney viscosity number or molecular weight on the performance of HNBR in NCM523 batteries is shown in samples 1, 4, 5 and 8, and the overall performance is equivalent to or slightly weaker than PVDF. Among them, the reversible capacity and capacity retention rate of sample 8 are better than PVDF. The reversible capacity of samples 1 and 5 in the first 120 weeks is higher, but the decay is faster in the later period. ③ HNBR binders with different ACN contents also have a certain effect on NCM523 batteries. Among them, although the reversible capacity of samples 6, 7 and 9 is lower than that of PVDF and sample 1, the cycle stability is better, especially sample 9 (the initial reversible capacity is 102mAh / g, and it remains at 121mAh / g after 200 cycles). From ①-③, we can conclude that in the NCM523 battery system, although the performance of each type of HNBR in reversible capacity and cycle stability is different, the overall performance has been significantly improved compared with the blank group. This shows that LiTFSI+LiDFOB has good applicability to various types of HNBR binders.
[0085] Example 9
[0086] Preparation and testing: Sample 1 was assembled into batteries with LFP, LCO and NCM523 materials respectively, and the effects of three addition methods of the modified components LiTFSI+LiDFOB on the battery performance were studied. The battery preparation and testing steps differ from those in Example 6 only in the electrode composition and the use of the modified components. The binder of this embodiment is sample 1, and the positive electrode active materials are LFP, LCO and NCM523. The use of the modified components is respectively an electrolyte additive, a binder solution, and a slurry composition, which is essentially the addition of the modified components at different stages of battery assembly. The specific operations are as follows.
[0087] Electrolyte additives: that is, adding modified components to the electrolyte, the mass ratio of LiTFSI and LiDFOB in the electrolyte to the mass ratio of lithium salt is 0.5%, and the total is 1.0%. The comparative example and Examples 1-8 of the present invention all adopt this scheme, which will not be repeated here.
[0088] Binder solution: 150 mg HNBR, 75 mg LiTFSI and 75 mg LiDFOB were dispersed in 4 mL NMP solvent and stirred at room temperature (20-30°C) for 6 h to obtain a uniform solution, i.e., the binder solution. When preparing the electrode, the binder solution was weighed according to the mass ratio of positive electrode material: binder: conductive carbon black 8:1:1, and no additional NMP was added. All operations were carried out in an argon protective atmosphere. A blank electrolyte was used during the battery test phase.
[0089] Slurry composition: 1200 mg of positive electrode active material, 150 mg of HNBR, 150 mg of carbon black, 75 mg of LiTFSI and 75 mg of LiDFOB were dispersed in 4 mL of NMP solvent, and magnetic high-speed stirring was performed at room temperature (20-30°C) for 6 h to obtain a uniform slurry. The slurry was evenly coated on the current collector during electrode preparation, and other operations were consistent with those described in the comparative example and Examples 1-8. All operations were carried out in an argon protective atmosphere. A blank electrolyte was used during the battery testing phase.
[0090] Performance description: Table 3 shows the effect of the use of LiDFOB / LiTFSI on the battery performance described in this example. It can be seen that the three use methods of the modified components all show excellent first-cycle capacity, first-cycle coulomb efficiency, first-cycle voltage difference and long-cycle capacity retention rate, among which the electrolyte additive method is more effective.
[0091] Table 3 Effect of the use of LiDFOB / LiTFSI in Example 9 on battery performance
[0092]
[0093] Example 10
[0094] Sample 1 was assembled into batteries with LFP, LCO and NCM523 materials respectively, and the effect of the usage of modified components LiTFSI+LiDFOB on the battery performance was studied.
[0095] Preparation and testing: The battery preparation and testing steps differ from those of Example 9 only in the use and amount of the modified component. The modified component of this example is LiTFSI+LiDFOB (1:1), and the use method is electrolyte additive. The total amount of the modified component used is 0.0%, 0.5%, 1.0% and 2.0% of the lithium salt.
[0096] Performance description: Table 4 shows the effect of the amount of the modified component used in this embodiment on the battery performance. It can be seen that the effect of the amount of the modified component used is manifested in three aspects. ① With the increase in the amount of the modified component, the first-week capacity of the three batteries LFP, LCO and NCM523 gradually increases (the first-week capacity of 0.0% and 0.5% in the NCM523 battery is basically the same), and the first-week voltage difference gradually decreases or remains the same, indicating that the modified component helps to improve the utilization rate of the active material and helps to reduce the electrode impedance. ② With the increase in the amount of the modified component, the first-week coulombic efficiency of the LFP battery first increases and then decreases, and the first-week coulombic efficiency of the LCO and NCM523 batteries gradually decreases. When the usage is 2.0%, the first-week coulombic efficiency of the three batteries is the lowest. The reduction in coulombic efficiency may be related to the formation of a new electrode / electrolyte interface film. ③ With the increase of the amount of modified components, the capacity retention rates of LFP, LCO and NCM523 batteries all showed an increase (0.0%→0.5%→1.0%) and then a decrease (1.0%→2.0%), indicating that the appropriate amount of modified components helps to improve the stability of battery cycles. Overall, the 1.0% addition has the greatest improvement on the comprehensive performance of LFP, LCO and NCM523 batteries.
[0097] Table 4 Effect of the amount of modified components used in Example 10 on battery performance
[0098]
[0099] Combined with Examples 1-10, the following four conclusions can be drawn from the comprehensive analysis. ① All HNBR samples showed obvious performance differences in the four electrolytes of LiTFSI+LiDFOB, LiTFSI, LiDFOB and blank group, among which LiTFSI+LiDFOB had the best performance, the blank group had the worst performance, and LiTFSI and LiDFOB had equivalent or mutual advantages and disadvantages. ② Although the ACN content, hydrogen saturation and Mooney viscosity number have different degrees of influence on the electrochemical performance of HNBR in the three positive electrode systems of LFP, LCO and NCM523, the core performance (reversible capacity, cycle performance and capacity retention rate) of most HNBR samples are better or equivalent to PVDF when the LiTFSI+LiDFOB modified component is present. This shows that the LiTFSI+LiDFOB proposed in the present invention has good applicability to various types of HNBR (involving a wide range of changes in ACN content, hydrogen saturation and Mooney viscosity number) and various positive electrode materials (such as LFP, LCO and NCM523). The reason for the modification may be that the modified components make up for the obvious deficiencies of traditional electrolytes in terms of lithium ion migration speed, stability and film-forming quality on the surface of active substances, and change the use environment of HNBR; in particular, the modified components realize pre-film formation on the active surface of the positive electrode, partially or completely isolating the surface of the active substance from HNBR, and realizing dual protection of the two, thereby significantly improving the battery capacity and stability. ③ The modified component scheme proposed in the present invention has a variety of effective use methods, which can be added in different forms at different stages of battery preparation, and all show excellent comprehensive performance. ④ When the addition amount of LiTFSI+LiDFOB modified components is 1.0% of the lithium salt, the comprehensive performance of the three batteries of LFP, LCO and NCM523 is improved the most.
[0100] The specific implementation contents described above are specific descriptions of the contents of the present invention in combination with preferred embodiments, but it cannot be determined that the specific implementation of the present invention is limited to the embodiments. For those skilled in the art who understand the field to which the present invention belongs, other evolutions and substitutions can be made without departing from the research ideas of the present invention, and these deductions and substitutions are all included in the scope defined by the claims of the present invention.
Claims
1. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte; Features: The positive electrode uses hydrogenated nitrile rubber as a binder, which is obtained by mixing a positive electrode active material, hydrogenated nitrile rubber, a conductive agent, and a solvent to form a positive electrode slurry, and then evenly coating the positive electrode slurry on a current collector and drying it; The hydrogenation saturation of the hydrogenated nitrile rubber is ≥90%; the acrylonitrile content is 16%-50%; the Mooney viscosity ML (1+4) @ 100°C is 20-85 or the molecular weight Mw is 20000-40000; The positive electrode slurry or electrolyte also contains a modified component, and the modified component is selected from one or more of lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate, fluoroethylene carbonate, lithium bis(oxalatoborate), and trifluoroethylphosphite.
2. The lithium ion battery according to claim 1, Features: The hydrogenation saturation of the hydrogenated nitrile rubber is ≥95%.
3. The lithium ion battery according to claim 2, Features: The hydrogenation saturation of the hydrogenated nitrile rubber is greater than 99%.
4. The lithium ion battery according to claim 1, Features: The acrylonitrile content of the hydrogenated nitrile rubber is 22%-40%.
5. The lithium ion battery according to claim 4, Features: The acrylonitrile content of the hydrogenated nitrile rubber is 26%-34%.
6. The lithium ion battery according to claim 5, Features: The acrylonitrile content of the hydrogenated nitrile rubber is 26%-29%.
7. The lithium ion battery according to claim 1, Features: The Mooney viscosity ML (1+4) @ 100°C of the hydrogenated nitrile rubber is 20-75.
8. The lithium ion battery according to claim 1, Features: The Mooney viscosity ML (1+4) @ 100°C of the hydrogenated nitrile rubber is 20-70.
9. The lithium ion battery according to claim 1, Features: The Mooney viscosity ML (1+4) @ 100°C of the hydrogenated nitrile rubber is 20-30.
10. The lithium ion battery according to claim 1, Features: The molecular weight Mw of the hydrogenated nitrile rubber is 30000-40000.
11. The lithium ion battery according to claim 1, Features: The positive electrode slurry contains a modified component, and the modified component is added by way a or way b: Method a: Under the protection of inert gas, HNBR and modified components are dispersed in a solvent, and the binder solution is obtained by fully dispersing the HNBR and modified components. Then, the lithium salt, the binder solution and the conductive agent are mixed evenly to obtain the positive electrode slurry; wherein the mass ratio of HNBR to the modified components is 1:0.5-2.0; Method b: Under the protection of inert gas, the positive electrode active material, hydrogenated nitrile rubber, conductive agent and modified component are directly mixed in a solvent and fully dispersed to obtain a positive electrode slurry; wherein the mass ratio of HNBR to the modified component is 1:0.5-2.0; Alternatively, the electrolyte further contains a modifying component, and the content of the modifying component is 0.5-2.0% of the amount of the lithium salt.
12. The lithium ion battery according to claim 11, Features: The electrolyte also contains a modified component, and the content of the modified component is 1% of the amount of lithium salt used.
Citation Information
Patent Citations
Low-temperature lithium iron phosphate battery and preparation method
CN106328938A
Lithium ion battery electrolyte solution
CN107749492A
Hydrogenated butyronitrile ester rubber, rubber material, vulcanized rubber and preparation method and application thereof
CN115785304A
Positive pole piece, secondary battery and electronic device
CN116111044A
Lithium ion battery, positive pole piece and electric device
CN118738285A
Cited By
Lithium battery pole piece containing cross-linked hydrogenated nitrile rubber binder and preparation method of lithium battery pole piece
CN119994002A
A lithium battery pole piece containing a cross-linked hydrogenated nitrile rubber binder and a preparation method thereof
CN119994002B
HNBR modified positive pole piece, positive current collector, diaphragm and lithium-air battery
CN122025667A