Lithium ion battery electrolyte with synergistic effect of rubidium / cesium and iodine

By adding rubidium/cesium and iodine ions to the lithium-ion battery electrolyte, an electrostatic shielding field is formed and dead lithium is activated, the problem of insufficient circulation performance and life of lithium-ion batteries is solved, and higher circulation performance and capacity retention rate are achieved .

CN118970186AInactive Publication Date: 2024-11-15ZIJIN MINING GROUP CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411050339.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cycling performance of existing lithium-ion batteries is affected by solid electrolyte interface film (SEI film) and lithium dendrites, resulting in a short battery life. The existing solution cannot completely inhibit the formation of lithium dendrites, resulting in the production of dead lithium.

Method used

Using a lithium-ion battery electrolyte that synergistically interacts rubidium/cesium and iodine, by adding rubidium ions, cesium ions and iodine ions to the electrolyte, a surface electrostatic shielding field is formed and dead lithium is activated, thereby reducing the growth of lithium dendrites and activate dead lithium. This improves the cycle life of the battery.

Benefits of technology

Through the synergistic action of rubidium/cesium and iodine ions, the cycle performance and life of lithium-ion batteries are significantly improved, polarization is reduced, and the capacity retention rate of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970186A_ABST
    Figure CN118970186A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium ion battery electrolyte with synergistic effect of rubidium / cesium and iodine. The lithium ion battery electrolyte is mainly prepared from an organic solvent, a lithium salt, an iodine-containing compound and a cesium-containing compound and / or a rubidium-containing compound. Due to the fact that rubidium ions / cesium ions have high electropositivity, the rubidium ions / cesium ions can be adsorbed on the surfaces of the protrusions in the lithium deposition process, a surface electrostatic shielding field is formed, and uniform deposition of lithium is guided. Therefore, by adding a small amount of rubidium ions / cesium ions, the cycle performance of the battery can be improved, and polarization is reduced. In addition, due to the fact that the iodide ions or the iodide triions have reducibility, dead lithium (lithium oxide) without activity can be converted into active lithium by introducing the iodide ions or the iodide triions. Therefore, the cycle life of the battery can be prolonged by adding a small amount of iodide ions or triiodide ions. Through the ion synergistic effect of rubidium ions / cesium ions and iodide ions / triiodide ions, lithium dendrite growth can be reduced, dead lithium can be activated, and the cycle life of the battery is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery electrolyte with synergistic effects of rubidium / cesium and iodine. Background Art

[0002] With the widespread application of renewable energy and the transformation and upgrading of energy structure, the importance of energy storage technology has become increasingly prominent. People are paying more and more attention to the field of energy storage, not only because it is of great significance to solving the energy crisis and promoting green development, but also because of the huge market potential and broad application prospects brought by energy storage technology. In recent years, lithium-ion batteries have been widely used in the field of energy storage, especially polyanion lithium-ion batteries, which have attracted people's attention due to their high safety, low cost and long cycle life. However, with the rapid update and iteration of secondary battery technology, people have put forward higher requirements for its cycle performance.

[0003] At present, polyanion lithium-ion positive electrode materials (such as lithium iron phosphate) are limited by the current technical level of lithium iron phosphate batteries, and the service life of some lithium iron phosphate energy storage systems is not long. Therefore, how to improve its cycle performance is the current research direction. Taking lithium iron phosphate as an example, the cycle performance of lithium iron phosphate is mainly affected by the solid electrolyte interface film (SEI film) and lithium dendrites. During the first charging process, the surface of the electrode material will react with the electrolyte to form a passivation layer, which is the SEI film. The quality of the SEI film will directly affect the performance of the battery. The ideal SEI film should have high ionic conductivity, thin and dense characteristics. In addition, the cycle life of lithium-ion batteries is also related to the growth of lithium dendrites. At high rates or overcharge conditions, lithium ions will aggregate and grow on the surface of the anode material to form lithium dendrites. The formation of lithium dendrites may pierce the diaphragm, causing a short circuit in the battery and leading to safety accidents. In addition, the breakage of lithium dendrites will lead to the generation of dead lithium, thereby affecting the capacity and service life of the battery.

[0004] People have also explored the above problems. For example, Chinese patent application CN114335722A discloses a lithium-ion battery, electrolyte and additives thereof, using fluorides of lithium, sodium, potassium, rubidium, cesium and francium to enhance the stability of the SEI film and improve the rate charge and discharge performance. Chinese patent application CN115842158A discloses an electrolyte and a preparation method thereof, a secondary battery, a battery module, a battery pack and an electrical device containing the electrolyte, using potassium ions, rubidium ions, cesium ions, barium ions and other ions to inhibit the growth of lithium dendrites, improve the retention of the battery cell cycle capacity, and extend the cycle life of the battery cell. Chinese patent application CN106450452A discloses a new use of rubidium-cesium compounds, high-voltage electrolyte additives, high-voltage electrolytes and lithium-ion batteries. The use of rubidium-cesium compounds as high-voltage electrolyte additives for lithium-ion batteries can protect the positive electrode material, effectively reduce the oxidative decomposition of the electrolyte on the positive electrode surface, greatly improve the cycle stability of the battery, and increase the battery life.

[0005] The above-mentioned schemes mainly utilize the electrostatic shielding effect of rubidium ions and cesium ions to reduce the formation of lithium dendrites and thus improve the cycle performance of lithium-ion batteries. However, even if a certain amount of rubidium and cesium ions are added to the electrolyte, the formation of lithium dendrites cannot be completely inhibited, thereby resulting in the generation of dead lithium. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a lithium-ion battery electrolyte with synergistic effects of rubidium / cesium and iodine.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A lithium-ion battery electrolyte with synergistic effects of rubidium / cesium and iodine is mainly made of an organic solvent, a lithium salt, an iodine-containing compound, and a cesium-containing compound and / or a rubidium-containing compound.

[0009] Furthermore, the rubidium-containing compound includes one or more of rubidium chloride, rubidium carbonate, rubidium nitrate, rubidium sulfate, rubidium acetate, rubidium tetrafluoroborate, rubidium hexafluorophosphate, rubidium bromide, rubidium iodide, rubidium perchlorate, rubidium tetraphenylborate, and rubidium bis(trifluoromethylsulfonyl)imide.

[0010] Further, the cesium-containing compound includes one or more of cesium chloride, cesium carbonate, cesium nitrate, cesium sulfate, cesium acetate, cesium perchlorate, cesium hexafluorophosphate, cesium bromide, cesium iodide, cesium triiodide, cesium methanesulfonate, and cesium bis(trifluoromethylsulfonyl)imide.

[0011] Furthermore, the iodine-containing compound includes one or more of sodium iodide, potassium iodide, rubidium iodide, cesium iodide, sodium triiodide, cesium triiodide, and ammonium triiodide.

[0012] Further, the cesium-containing compound and / or the rubidium-containing compound does not contain iodide ions and the iodine-containing compound does not contain cesium and / or rubidium, or the rubidium-containing compound and / or the cesium-containing compound uses rubidium iodide and / or cesium iodide, and the rubidium iodide and / or cesium iodide simultaneously serve as the iodine-containing compound.

[0013] Furthermore, the added concentration of the rubidium-containing compound is 0.005-0.1 mol / L.

[0014] Furthermore, the added concentration of the cesium-containing compound is 0.005-0.1 mol / L.

[0015] Furthermore, the added concentration of the iodine-containing compound is 0.005-0.1 mol / L.

[0016] Further, the organic solvent includes one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl formate, tetrahydrofuran, 2-methyl-tetrahydrofuran, 2-methyl-tetrahydrofuran, and acetonitrile; the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(perfluoroethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium bis(oxalatoborate).

[0017] The present invention also provides a method for preparing the above-mentioned lithium ion battery electrolyte with synergistic effect of rubidium / cesium and iodine, comprising the following steps:

[0018] Step 1: In a dry glove box filled with argon, add lithium salt to an organic solvent and stir to dissolve, to obtain an electrolyte without adding additives;

[0019] Step 2: In the glove box, add an iodine-containing compound and a rubidium-containing compound and / or a cesium-containing compound to the electrolyte obtained in step 1, and stir and dissolve to obtain a lithium-ion battery electrolyte with synergistic effects of rubidium / cesium and iodine.

[0020] The beneficial effect of the present invention is that the electrolyte prepared by the present invention contains rubidium / cesium ions and iodine ions / triiodine ions. Among them, since the rubidium ions / cesium ions have strong positive charge, they can be adsorbed on the surface of the protrusions during the lithium deposition process to form a surface electrostatic shielding field and guide the uniform deposition of lithium. Therefore, adding a small amount of rubidium ions / cesium ions can improve the cycle performance of the battery and reduce polarization. In addition, since iodine ions or triiodine ions are reducing, inactive dead lithium (lithium oxide) can be converted into active lithium by introducing iodine ions or triiodine ions. Therefore, adding a small amount of iodine ions or triiodine ions can improve the cycle life of the battery. The present invention can reduce the growth of lithium dendrites and activate dead lithium through the ionic synergistic effect of rubidium ions / cesium ions and iodine ions / triiodine ions, and the cycle life of the battery is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a graph of the cycle capacity retention rates of Example 10, Comparative Example 1 and Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0022] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.

[0023] Example 1

[0024] In a dry glove box filled with 99.999% argon, ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were first mixed in a volume ratio of 1:1:1 and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L rubidium tetrafluoroborate and 0.02 mol / L sodium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of rubidium and iodine.

[0025] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery:

[0026] Preparation of positive electrode: lithium iron phosphate, carboxymethyl cellulose (CMC), and styrenated phenol (SP) were mixed in a mass ratio of 8:1:1, and then NMP was added and stirred evenly. Then, the mixture was coated on aluminum foil, dried, and cut into small discs with a diameter of 14 mm.

[0027] Preparation of negative electrode: artificial graphite, SP, CMC, and styrene-butadiene rubber (SBR) were mixed evenly in a mass ratio of 95.5:1.5:1.2:1.8, and then deionized water was added to mix evenly, coated on copper foil, and cut into small discs with a diameter of 16 mm after drying.

[0028] The positive electrode sheet and the negative electrode sheet were transferred to the glove box, and a 25 μm thick 19 mm diameter PP separator was used to assemble the CR2032 button battery in the order of negative electrode shell, spring, gasket, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell.

[0029] Example 2

[0030] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6The mixture is stirred and dissolved, and then 0.02 mol / L cesium hexafluorophosphate and 0.02 mol / L sodium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0031] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0032] Example 3

[0033] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L rubidium perchlorate and 0.02 mol / L cesium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte having a synergistic effect of rubidium, cesium and iodine.

[0034] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0035] Example 4

[0036] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L cesium perchlorate and 0.02 mol / L cesium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0037] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0038] Example 5

[0039] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and 0.02 mol / L cesium triiodide is added and stirred and dissolved to obtain a lithium-ion battery electrolyte having a synergistic effect of cesium and iodine.

[0040] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0041] Example 6

[0042] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L rubidium tetrafluoroborate and 0.02 mol / L potassium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of rubidium and iodine.

[0043] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0044] Example 7

[0045] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L cesium hexafluorophosphate and 0.02 mol / L potassium iodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0046] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0047] Example 8

[0048] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L rubidium tetrafluoroborate, 0.02 mol / L cesium hexafluorophosphate, and 0.02 mol / L sodium triiodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium, rubidium, and iodine.

[0049] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0050] Example 9

[0051] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.005 mol / L cesium hexafluorophosphate and 0.005 mol / L sodium triiodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0052] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0053] Example 10

[0054] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L cesium hexafluorophosphate and 0.02 mol / L sodium triiodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0055] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0056] Embodiment 11

[0057] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.04 mol / L cesium hexafluorophosphate and 0.04 mol / L sodium triiodide are added and stirred and dissolved to obtain a lithium-ion battery electrolyte with synergistic effects of cesium and iodine.

[0058] The lithium ion battery electrolyte of this embodiment is used to prepare a polyanion lithium ion button battery according to the method of embodiment 1.

[0059] Comparative Example 1

[0060] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L cesium hexafluorophosphate is added and stirred and dissolved to obtain a cesium-containing lithium-ion battery electrolyte.

[0061] The lithium ion battery electrolyte of this comparative example was used to prepare a polyanion lithium ion button battery according to the method of Example 1.

[0062] Comparative Example 2

[0063] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 The mixture is stirred and dissolved, and then 0.02 mol / L rubidium tetrafluoroborate is added and stirred and dissolved to obtain a lithium-ion battery electrolyte containing rubidium.

[0064] The lithium ion battery electrolyte of this comparative example was used to prepare a polyanion lithium ion button battery according to the method of Example 1.

[0065] Comparative Example 3

[0066] In a dry glove box filled with 99.999% argon, firstly, EC, DMC, and EMC were mixed evenly at a volume percentage of 1:1:1, and then 1 mol / L LiPF 6 Stir and dissolve to obtain a lithium ion electrolyte.

[0067] The lithium ion battery electrolyte of this comparative example was used to prepare a polyanion lithium ion button battery according to the method of Example 1.

[0068] The 11 embodiments and 3 comparative examples were subjected to charge and discharge tests, with a charge cut-off voltage of 3.8 V and a discharge cut-off voltage of 2 V. The capacity retention rate after 1000 cycles at 1C is shown in Table 1.

[0069] Table 1

[0070]

[0071]

[0072] From the data in Table 1, it can be seen that the capacity retention rates of Examples 1-11 in which rubidium / cesium ions and iodine ions are added to the electrolyte after 1000 cycles at 1C are higher than those of Comparative Example 3 in which no composite additive is added and Comparative Examples 1-2 in which only a single rubidium compound or a single cesium compound is added. Figure 1 This is a cycle capacity retention rate graph of Example 10, Comparative Example 1 and Comparative Example 3. It can be seen that Example 10 to which cesium ions and iodide ions are added has the highest capacity retention rate after 1000 cycles at 1C, while Comparative Example 1 to which a single cesium compound is added has the second highest capacity retention rate, and Comparative Example 3 to which no additives are added has the worst performance, indicating that the composite additives have a synergistic effect, and the composite additives have a more significant improvement on the battery cycle.

[0073] In summary, the addition of rubidium / cesium ions and iodide ions can play an ionic synergistic role in reducing the growth of lithium dendrites and activating dead lithium, thereby improving the cycle life of the battery.

[0074] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.

Claims

1. A lithium ion battery electrolyte with synergistic effects of rubidium / cesium and iodine, characterized in that: It is mainly made of organic solvent, lithium salt, iodine-containing compound and cesium-containing compound and / or rubidium-containing compound.

2. The lithium ion battery electrolyte according to claim 1, characterized in that: The rubidium-containing compound includes one or more of rubidium chloride, rubidium carbonate, rubidium nitrate, rubidium sulfate, rubidium acetate, rubidium tetrafluoroborate, rubidium hexafluorophosphate, rubidium bromide, rubidium iodide, rubidium perchlorate, rubidium tetraphenylborate, and rubidium bis(trifluoromethylsulfonyl)imide.

3. The lithium ion battery electrolyte according to claim 1, characterized in that The cesium-containing compound includes one or more of cesium chloride, cesium carbonate, cesium nitrate, cesium sulfate, cesium acetate, cesium perchlorate, cesium hexafluorophosphate, cesium bromide, cesium iodide, cesium triiodide, cesium methanesulfonate, and cesium bis(trifluoromethylsulfonyl)imide.

4. The lithium ion battery electrolyte according to claim 1, characterized in that: The iodine-containing compound includes one or more of sodium iodide, potassium iodide, rubidium iodide, cesium iodide, sodium triiodide, cesium triiodide, and ammonium triiodide.

5. The lithium ion battery electrolyte according to claim 1, characterized in that: The cesium-containing compound and / or the rubidium-containing compound does not contain iodide ions and the iodine-containing compound does not contain cesium and / or rubidium, or the rubidium-containing compound and / or the cesium-containing compound uses rubidium iodide and / or cesium iodide, and the rubidium iodide and / or cesium iodide simultaneously serve as the iodine-containing compound.

6. The lithium ion battery electrolyte according to claim 1, characterized in that: The added concentration of the rubidium-containing compound is 0.005-0.1 mol / L.

7. The lithium ion battery electrolyte according to claim 1, characterized in that: The added concentration of the cesium-containing compound is 0.005-0.1 mol / L.

8. The lithium ion battery electrolyte according to claim 1, characterized in that: The added concentration of the iodine-containing compound is 0.005-0.1 mol / L.

9. The lithium ion battery electrolyte according to claim 1, characterized in that: The organic solvent includes one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl formate, tetrahydrofuran, 2-methyl-tetrahydrofuran, 2-methyl-tetrahydrofuran, and acetonitrile; the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(perfluoroethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium bis(oxalatoborate).

10. A method for preparing the lithium-ion battery electrolyte with synergistic effects of rubidium / cesium and iodine according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: In a dry glove box filled with argon, add lithium salt to an organic solvent and stir to dissolve, to obtain an electrolyte without adding additives; Step 2: In the glove box, add an iodine-containing compound and a rubidium-containing compound and / or a cesium-containing compound to the electrolyte obtained in step 1, and stir and dissolve to obtain a lithium-ion battery electrolyte with synergistic effects of rubidium / cesium and iodine.

Citation Information

Patent Citations

  • Lithium-ion rechargeable battery

    CN103140980A

  • New use of rubidium cesium compound, high-voltage electrolyte additive, high-voltage electrolyte and lithium ion battery

    CN106450452A

  • Lithium ion battery and method for photo-assisted activation of dead lithium

    CN113782815A

  • Multifunctional lithium battery additive containing fluorine and boron element substances and application of multifunctional lithium battery additive

    CN114824468A

  • Electrolyte additive as well as preparation method and application thereof

    CN116315085A