Ultrathin, flame-retardant and electrically-insulating aramid nanofiber diaphragm and application thereof
By converting aramid microfibers into ultra-thin, flame-retardant, electrically insulated nanofiber separators, the problem of growth and corrosion of zinc negative electrode dendrites in aqueous zinc ion batteries is solved, and the cycle stability and energy density of the battery are improved, thus achieving the realization of the battery. Efficient macroscopic preparation of diaphragms.
Patent Information
- Application Number
- CN202410933864.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing aqueous zinc ion batteries lack separators with small thickness, high mechanical strength, uniform pore size distribution, rich functional polar groups, flame retardant and low cost, resulting in dendrite growth and corrosion problems in the battery, affecting circulation. Stability and reversibility.
Ultrasonic treatment and vacuum-assisted suction filtration technology are used to convert aramid microfiber fibers into ultra-thin, flame-retardant, electrically insulated nanofiber membranes. The layered porous structure membrane is obtained through solvent exchange dilution and drying, which regulates the zinc ion deposition orientation and reduces the Cutting edge effect.
It improves the reversibility and energy density of zinc negative electrodes of zinc ion batteries, enhances the tensile strength and heat resistance of the separator, reduces the cost of the battery, and is suitable for macro-preparation.
Smart Images

Figure CN118970372A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nano material preparation, and specifically relates to an ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm and application thereof. Background Art
[0002] The intensification of the energy crisis and the demand for large-scale energy storage have promoted the development of advanced renewable energy technologies. Although lithium-ion batteries have been successful in the commercial fields of portable electronics and new energy vehicles, limited lithium resource reserves, high costs and serious safety hazards have restricted their application in the field of large-scale energy storage. Therefore, it is crucial to explore low-cost and high-safety energy storage systems. Aqueous zinc-ion batteries, such as aqueous zinc-ion batteries, have good application prospects in the field of large-scale energy storage power sources due to their abundant resources, low cost and high safety.
[0003] Currently, there is a lack of standardized and practical separators for electrochemical evaluation of aqueous zinc-ion batteries, similar to polypropylene separators in lithium-ion batteries. The glass fiber separators commonly used in aqueous zinc-ion batteries have large pore sizes, are too thick, and have unsatisfactory mechanical properties. Therefore, it is urgent to find a high-performance separator with small thickness, high mechanical strength, relatively uniform pore size distribution, functional polar groups, flame retardancy, low cost, and mass production.
[0004] Zinc (Zn) metal anodes face severe challenges of dendrite growth and continuous corrosion in aqueous electrolytes, which seriously affect the cycle stability and reversibility of the battery. The electrodeposition behavior of zinc is mainly affected by the electric field distribution and the orientation of the deposited crystals. The inherent inhomogeneity of the surface of the zinc metal anode leads to the irregular distribution of the electric field, which promotes the Zn 2+ Ions are preferentially electrodeposited in the tip region ("tip effect"). Zinc metal exhibits a close-packed hexagonal crystal structure, and the Zn(002) crystal plane has a more uniform surface atomic arrangement and interface charge density compared to the Zn(100) and Zn(101) crystal planes, which is conducive to achieving uniform Zn 2+ The Zn(002) crystal plane also has stronger corrosion resistance than the Zn(100) and Zn(101) crystal planes. Therefore, regulating the Zn deposition orientation provides a promising method for obtaining highly stable and reversible Zn metal anodes.
[0005] Aromatic polyamide fiber (aramid for short) refers to a type of synthetic fiber made from linear polyamide containing aromatic rings. It is divided into fully aromatic polyamide fiber and aliphatic polyamide fiber containing aromatic rings, mainly poly(p-phenylene terephthalamide) fiber and poly(m-phenylene isophthalamide) fiber. In addition, there are poly(p-phenylene terephthalamide) fiber, etc. Aramid fiber has excellent heat resistance, chemical corrosion resistance, flame retardancy, electrical insulation performance and other characteristics, and is widely used in many fields. Summary of the invention
[0006] In view of the above problems, the present invention aims to provide an ultra-thin, flame-retardant, electrically insulating high-performance aramid nanofiber diaphragm with small thickness (less than 20 μm, especially less than 10 μm), high mechanical strength, relatively uniform pore size distribution, low cost, and easy mass production, and is applied to the mass production of aqueous zinc ion batteries to improve the reversibility and energy density of the zinc negative electrode of aqueous zinc ion batteries while improving the zinc utilization rate. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm has abundant polar functional groups, interconnected nanopores, high porosity, high mechanical strength, excellent heat resistance, flame retardancy and electrical insulation properties.
[0007] In a first aspect, the present invention provides a method for preparing an ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator, comprising the following steps: (1) mixing aramid micron fibers with dimethyl sulfoxide and potassium hydroxide aqueous solution to obtain aramid micron fiber slurry; (2) diluting the obtained aramid micron fiber slurry several times by solvent exchange, and ultrasonically treating the aramid nanofiber slurry; (3) The obtained aramid nanofiber slurry is subjected to vacuum-assisted filtration and drying to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane.
[0008] Preferably, in step (1), the aramid micron fiber has a diameter of 1 to 20 μm and a length of 1 to 5 mm.
[0009] Preferably, in step (1), the mass / volume ratio of the aramid micron fiber to the potassium hydroxide aqueous solution is 1 g: (5-20) mL; Preferably, the molar concentration of the potassium hydroxide aqueous solution is 0.1 to 10 mol L -1 .
[0010] Preferably, in step (1), the volume ratio of the potassium hydroxide aqueous solution to dimethyl sulfoxide is 1:(1-200), preferably 1:(25-100).
[0011] Preferably, the aramid micron fiber slurry is stirred before solvent exchange and dilution; the stirring time is 3 to 72 hours; Preferably, the exchange solvent is ethanol; the solvent exchange dilution multiple is 1 to 10.
[0012] Preferably, in step (2), the parameters of the ultrasonic treatment include: power of 200 to 800 W, and time of 10 to 60 min.
[0013] Preferably, in step (3), the parameters of the vacuum-assisted filtration include: dividing the aramid nanofiber slurry into two, filtering the first portion of the aramid nanofiber slurry, rotating the filtration bottle horizontally by 180°, adding the second portion of the aramid nanofiber slurry for filtration, and adding deionized water to the filtration bottle for multiple washing after the filtration is completed. The present invention uses the above vacuum-assisted filtration process to ensure the uniformity of the thickness of the ultra-thin aramid nanofiber diaphragm.
[0014] Preferably, the drying temperature is 80-120° C. and the drying time is 20-60 min.
[0015] In the second aspect, the present invention provides an ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane prepared according to the above-mentioned preparation method, wherein the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is a layered, porous structure formed by interweaving and stacking electronegative aramid nanofibers; the diameter of the aramid nanofiber is 1 to 20 nm, and the length is 1 to 100 μm; the zeta potential of the aramid nanofiber is -25 to -45 mV.
[0016] Preferably, the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane has a thickness of 2 to 20 μm, preferably 5 to 10 μm.
[0017] Preferably, in the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane, the pore size of the porous structure is 100 to 250 nm.
[0018] Preferably, the tensile strength of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is 110-130 MPa; the Young's modulus of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is 40-50 GPa.
[0019] In a third aspect, the present invention also provides an aqueous zinc ion battery comprising the above-mentioned ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane.
[0020] The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared by the present invention has a uniform pore size distribution and can provide a uniform zinc ion flux in an aqueous zinc ion battery. The aramid nanofiber diaphragm has good tensile strength and Young's modulus, and can resist damage that may be caused by zinc dendrites. The aramid nanofiber diaphragm contains carbonyl (-C=O) and amino (-NH2) polar groups in the smallest polymer unit, which can change the solvation of zinc ions, accelerate the desolvation process of zinc ions, and enhance the zinc ion transfer kinetics. The uniformly distributed nanopores in the aramid nanofiber diaphragm effectively regulate the distribution of zinc ions at the diaphragm-zinc negative electrode interface, uniformize the zinc ion flux and electric field distribution, and thus reduce the tip effect. The aramid nanofiber diaphragm can promote the deposition of zinc ions along the two directions of Zn (100) and Zn (101), slow down the growth rate of the Zn (002) crystal plane, thereby exposing more Zn (002) textures and preventing the formation of zinc dendrites. Therefore, the aqueous zinc ion battery assembled with the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared by the present invention can significantly improve the reversibility and energy density of the zinc negative electrode of the aqueous zinc ion battery while improving the zinc utilization rate.
[0021] Beneficial effects: The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared by the present invention has a small thickness (less than 20 μm, especially less than 10 μm), low cost, and is easy to prepare in batches; it has abundant polar functional groups, interconnected nanopores, relatively uniform pore size distribution, high porosity, high mechanical strength (tensile strength greater than 100 MPa), good heat resistance, and excellent flame retardant and electrical insulating properties. It is suitable for the large-scale preparation of aqueous zinc ion batteries and can effectively improve the utilization rate, reversibility and energy density of zinc electrodes in aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a digital photo of the aramid nanofiber slurry prepared in Example 1; Figure 2 TEM image (a) of the aramid nanofiber prepared by the present invention and diameter statistics of the aramid nanofiber (b); Figure 3 A digital photo (a) of an ultra-thin, flame-retardant, electrically insulating ultra-thin aramid nanofiber diaphragm sample with a diameter of 20 cm prepared in Example 1, a SEM image of the diaphragm surface (b), and the pore size distribution of the aramid nanofibers (c); Figure 4 Digital photograph (a) of the thickness of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm sample prepared in Example 1 measured by a screw micrometer, a SEM image of the diaphragm cross section (b), and a magnified SEM image of the diaphragm cross section (c); Figure 5The surface mass measurement of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator sample prepared in Example 1; Figure 6 The contact angle test of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane sample prepared in Example 1; Figure 7 The electrolyte absorption rate and retention rate of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator sample prepared in Example 1; Figure 8 Mechanical properties of the ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm (dry state) sample prepared in Example 1: (a) stress-strain curve of the diaphragm; (b) tensile strength and Young's modulus of the diaphragm; (c) digital photo of the diaphragm lifting a heavy object; Fig. 9 Mechanical properties of the ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm (wet state) sample prepared in Example 1: (a) stress-strain curve of the diaphragm; (b) tensile strength and Young's modulus of the diaphragm; Fig.10 Demonstration of the flexibility of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator sample prepared in Example 1; Fig.11 Cycling performance of a symmetrical battery prepared using the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator prepared in Example 1 under different conditions: (a) 5 mA cm -2 / 2.5mAh cm -2 (b) 10 mA cm -2 / 5mAh cm -2 ; Fig.12 Cycling performance of an asymmetric battery prepared using the ultrathin, flame-retardant, electrically insulating aramid nanofiber separator prepared in Example 1 under different conditions: (a) 1 mA cm -2 / 1mAh cm -2 (b) 2 mA cm -2 / 2mAh cm -2 ; Fig.13 The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (10 mg cm -2 ) Rate cycling performance of the full battery; Fig.14 The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (10 mg cm -2 ) Long cycle performance evaluation of full batteries; Fig.15 The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (15 mg cm-2 ) Evaluation of the long cycle performance of the full battery and calculation of the energy density based on the positive and negative electrode active materials and the separator (b); Fig.16 The digital photo of the ultrathin, flame-retardant, electrically insulating ultrathin aramid nanofiber membrane sample prepared in Example 4 (a) and the symmetrical battery prepared with the ultrathin aramid nanofiber membrane at 5 mA cm -2 / 2.5mAh cm -2 Cycling performance under the following conditions (b). DETAILED DESCRIPTION
[0023] To further explain the content, characteristics and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific embodiments. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention. In the absence of special instructions, each percentage refers to the percentage by mass.
[0024] The present invention prepares the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane by gradually peeling off aramid micron fibers from top to bottom into aramid nanofibers, and then vacuum filtration. The aramid nanofiber membrane is a layered porous structure formed by aramid nanofibers interwoven and stacked with each other, and its thickness is adjustable, preferably 2 to 20 μm, preferably 5 to 10 μm; in the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane, the pore size of the porous structure is 100 to 250 nm.
[0025] The following is an exemplary description of the method for preparing the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator provided by the present invention.
[0026] Preparation of aramid micron fiber slurry: The washed aramid micron fiber is mixed with dimethyl sulfoxide and potassium hydroxide aqueous solution to obtain aramid micron fiber slurry.
[0027] In an optional embodiment, the diameter of the aramid micron fiber is 1 to 20 μm and the length is 1 to 5 mm. The mass volume ratio of the aramid micron fiber to the potassium hydroxide aqueous solution is 1 g: (5 to 20) mL. The molar concentration of the potassium hydroxide aqueous solution is 0.1 to 10 mol L -1 The volume ratio of the potassium hydroxide aqueous solution to dimethyl sulfoxide is 1:(1-200), preferably 1:(25-100).
[0028] Preparation of aramid nanofiber slurry: After the obtained aramid micron fiber slurry is stirred for a certain period of time, it is diluted several times by solvent exchange and ultrasonically treated to obtain aramid nanofiber slurry.
[0029] In an optional embodiment, the stirring time is 3 to 72 hours. The solvent used is ethanol; the solvent exchange dilution multiple is 1 to 10. The parameters of the ultrasonic treatment include: power of 200 to 800 W, time of 10 to 60 min.
[0030] The obtained aramid nanofiber slurry is subjected to vacuum-assisted filtration and drying and the filter membrane is removed to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm.
[0031] In an optional embodiment, the vacuum-assisted filtration step is: divide the aramid nanofiber slurry into two parts, filter the first part of the aramid nanofiber slurry, rotate the filtration bottle 180° horizontally, add the second part of the aramid nanofiber slurry for filtration, and add deionized water to the filtration bottle for washing multiple times after the filtration is completed.
[0032] In an optional embodiment, the drying temperature is 80-120° C. and the drying time is 20-60 min.
[0033] The present invention uses a thickness tester to measure the thickness of the battery diaphragm, randomly takes 3 points on the diaphragm for measurement, and calculates the average value. A universal mechanical testing machine (Drick, DRK-101B) is used to test the tensile strength of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm. Specifically, the diaphragm is cut into a rectangular sample with a length of 40 mm and a width of 15 mm, and the two ends of the rectangular sample are clamped on the universal mechanical testing machine for tensile strength testing. The moving speed of the clamp is 5 mm / min, and the distance between the clamps is 10 mm. Electrolyte adsorption rate: The battery diaphragm is immersed in an electrolyte (the electrolyte is 3MZn(CF3SO3)2 with a concentration of 5M, and the solvent is deionized water for 5 minutes, and then calculated according to the following formula: Electrolyte adsorption rate (%) = (M-M0) / M0×100%; wherein, M0 is the initial weight of the diaphragm, and M is the weight of the diaphragm after adsorbing the electrolyte. Measure 3 times respectively and calculate the average value.
[0034] The ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane prepared by the present invention has a thickness of 2-20 μm, preferably 5-10 μm. In the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane, the pore size of the porous structure is 100-250 nm.
[0035] The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared by the present invention has a tensile strength of 110 to 130 MPa; the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm has a Young's modulus of 40 to 50 GPa.
[0036] The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared by the present invention can be applied to aqueous zinc ion batteries, including symmetrical batteries, non-symmetrical batteries and full batteries.
[0037] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0038] Example 1 (1) First, add 10 ml of potassium hydroxide aqueous solution (0.67 M) to 500 ml of dimethyl sulfoxide and mix well; (2) Then, 1 g of the washed aramid micron fiber was added to the solution containing the above solution and stirred vigorously for 24 hours to obtain an aramid fiber slurry; (3) Then, the obtained aramid fiber slurry was further diluted 4 times with ethanol and ultrasonically treated for 30 minutes to obtain the aramid nanofiber slurry; (4) Finally, in order to ensure the uniformity of the thickness of the ultra-thin aramid nanofiber diaphragm, 20 mL of aramid nanofiber slurry was taken and divided into two parts. After the first part of the aramid nanofiber slurry was filtered, the filtration bottle was rotated 180° horizontally, and the second part of the aramid nanofiber slurry was added for filtration. After the filtration was completed, deionized water was added to the filtration bottle for washing several times to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm.
[0039] Figure 1 This is a digital photo of the aramid nanofiber slurry prepared in Example 1. As can be seen from the figure, the aramid nanofibers are in a uniformly dispersed state after solvent exchange and ultrasonic dispersion.
[0040] Figure 2 The TEM image (a) and the diameter statistics (b) of the aramid nanofibers prepared in Example 1. As can be seen from the figure, the aramid nanofibers have a smaller diameter and a larger aspect ratio.
[0041] Figure 3The digital photo (a) of the ultra-thin, flame-retardant, electrically insulating ultra-thin aramid nanofiber diaphragm sample with a diameter of 20 cm prepared in Example 1, the SEM image of the diaphragm surface (b) and the pore size distribution of the aramid nanofiber (c). As can be seen from the figure, the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm is transparent light yellow. The surface of the aramid nanofiber diaphragm is formed by the aramid nanofibers interweaving to form a nanoscale porous structure with high porosity, and these nanoscale pores are uniformly distributed. The pore size distribution range of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm measured by the bubble pressure method is relatively narrow, and more than 90% of the pores are concentrated in the range of 100 to 300 nm. The statistical average pore size of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm is about 226 nm.
[0042] Figure 4 The digital photo (a), SEM image (b), and SEM magnified image (c) of the membrane cross section of the ultrathin, flame-retardant, and electrically insulating aramid nanofiber diaphragm sample prepared in Example 1 measured by a micrometer screw are shown. The thickness of the aramid nanofiber diaphragm sample measured by a micrometer screw is about 5 μm, and the cross section of the aramid nanofiber diaphragm presents an ordered layered structure.
[0043] Figure 5 The surface mass of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane sample prepared in Example 1 was measured. The surface mass of the aramid nanofiber membrane sample obtained in Example 1 was 0.8 mg cm -2 .
[0044] Figure 6 This is a contact angle test of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane sample prepared in Example 1. The contact angle of the aramid nanofiber membrane sample obtained in Example 1 is 56.5°, and the contact angle value is lower than 90°, indicating that the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is hydrophilic.
[0045] Figure 7 The electrolyte absorption rate and retention rate of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm sample prepared in Example 1. As can be seen from the figure, the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 has a high electrolyte adsorption rate, with a maximum electrolyte adsorption rate of 590%; after being placed in a constant temperature and humidity chamber (temperature of 25°C, relative humidity of 60%) for 24 hours, the electrolyte retention rate of the aramid nanofiber diaphragm is 70.8%, which can meet actual requirements.
[0046] Figure 8Mechanical properties of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm (dry state) sample prepared in Example 1: (a) stress-strain curve of the diaphragm; (b) tensile strength and Young's modulus of the diaphragm; (c) digital photo of the diaphragm lifting a heavy object. As can be seen from the figure, the tensile strength and Young's modulus of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 are very high, 117.8MPa and 41.6GPa respectively. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm with a width of 15mm can lift a weight of 1kg.
[0047] Fig. 9 Mechanical properties of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator (wet state) sample prepared in Example 1: (a) stress-strain curve of the separator; (b) tensile strength and Young's modulus of the separator. In the presence of electrolyte, the tensile strength and Young's modulus of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator prepared in Example 1 are both very high, 108.2 MPa and 30.9 GPa, respectively.
[0048] Fig.10 The flexibility of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane sample prepared in Example 1 is shown. As can be seen from the figure, the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane prepared in Example 1 can remain intact during the folding and rubbing process without obvious damage.
[0049] Battery performance test
[0050] Symmetrical battery assembly: Two pieces of zinc foil with the same diameter were placed on the upper and lower sides of the ANF separator, and 3MZn(CF3SO3)2 electrolyte was added. The cells were packaged into 2025 button cells for testing.
[0051] Fig.11 The cycle performance of the symmetrical battery prepared with the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator prepared in Example 1 under different conditions. Under working conditions close to the actual aqueous zinc ion, at 5 mA cm -2 / 2.5mAh cm -2 Under the condition, it can cycle for 850 hours; at 10mAcm -2 / 5mAh cm -2 The zinc anode with aramid nanofiber separator has a stable stripping / plating behavior.
[0052] Assembly of asymmetric cells: Zinc foil and copper foil of the same diameter were placed on the upper and lower sides of the ANF separator, and 3M Zn(CF3SO3)2 electrolyte was added, and packaged into 2025 button cells for testing. Coulombic efficiency represents the reversibility of zinc stripping / deposition and is considered to be an important parameter that directly affects the cycle life of the battery. Therefore, the effect of aramid nanofiber separator on zinc stripping / deposition Coulombic efficiency was evaluated as follows.
[0053] Fig.12 The cycle performance of the asymmetric battery prepared by using the ultra-thin, flame-retardant, electrically insulating aramid nanofiber separator prepared in Example 1 under different conditions. -2 / 1mAh cm -2 Under the condition of 2mAcm, it can be cycled for 1400 times, with an average coulombic efficiency of 99.22%; -2 / 2mAh cm -2 Under the same conditions, it can be cycled for 500 times with an average Coulomb efficiency of 99.47%, indicating that the aramid nanofiber separator can significantly improve the reversibility of the zinc deposition / stripping process, which will help improve the energy efficiency of the battery.
[0054] Preparation and assembly of full batteries: In order to demonstrate the practical application potential of aramid nanofiber separators, a high loading (~10 mg cm -2 and ∼15 mg cm -2 )Mn 2.5 V 10 O 24 ·5.9H2O (MVOH) as the positive electrode, thin zinc foil (50 μm and 30 μm) as the negative electrode, placed on the upper and lower sides of the aramid nanofiber separator, and a small amount of 3M Zn(CF3SO3)2+0.1MMnSO4 electrolyte (8.0 μL mAh -1 and 6.0 μL mAh -1 ), packaged into 2025 button cells for testing.
[0055] Fig.13 The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (10 mg cm -2 ) The rate cycling performance of the full battery. As can be seen from the figure, at a current density of 0.1A g -1 The initial specific capacity of the full battery is as high as 434.9 mAh g -1 ; When the current density increases to 1A g -1 The initial specific capacity of the full battery is as high as 373.8 mAh g -1 .
[0056] Fig.14The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (10 mg cm -2 ) Long cycle performance evaluation of the full battery. As can be seen from the figure, under the actual working conditions close to the aqueous zinc ion battery, the thickness of the zinc negative electrode is 50μm, the calculated N / P ratio is about 6.59, the amount of electrolyte is also controlled at a low level, and the electrolyte volume / capacity (E / C) ratio is 8.0μL mAh -1 After 300 cycles, the battery surface capacity can still be maintained at 3 mAh cm -2 The above figure is comparable to that of current commercial lithium-ion batteries, highlighting its great potential in practical applications, with a capacity retention rate of 80.7%.
[0057] Fig.15 The ultrathin, flame-retardant, electrically insulating aramid nanofiber diaphragm prepared in Example 1 was used to prepare a high-capacity (15 mg cm -2 ) Long cycle performance evaluation of the full battery and energy density calculation based on the positive and negative electrode active materials and the separator (b). As can be seen from the figure, the thickness of the zinc negative electrode is 30μm, the calculated N / P ratio is about 2.64, and the electrolyte volume / capacity (E / C) ratio is 6.0μL mAh -1 After 200 cycles, the surface capacity of the battery is 3.82 mAh cm -2 The capacity retention rate is 66.1%. Considering the positive and negative active materials and the separator, the ultra-thin aramid nanofiber separator occupies less space and mass (0.56mm 3 and 0.9 mg), the calculated mass energy density and volume energy density are 129.2 Wh kg -1 and 142.5Wh L -1 In the current context of the ultimate pursuit of battery energy density, aramid nanofiber separators have shown significant advantages.
[0058] Example 2 (1) First, add 7.5 ml of potassium hydroxide aqueous solution (0.67 M) to 500 ml of dimethyl sulfoxide and mix well; (2) Then, 1 g of the washed aramid fiber was added to the above solution and stirred vigorously for 24 hours to obtain an aramid nanofiber stock solution; (3) Then, the obtained aramid micron fiber stock solution was further diluted 4 times with ethanol and ultrasonically treated for 30 minutes to obtain the aramid nanofiber slurry; (4) Finally, in order to ensure the uniformity of the thickness of the ultra-thin aramid nanofiber diaphragm, 20 mL of aramid nanofiber slurry was taken and divided into two parts. After the first part of the aramid nanofiber slurry was filtered, the filtration bottle was rotated 180° horizontally, and the second part of the aramid nanofiber slurry was added for filtration. After the filtration was completed, deionized water was added to the filtration bottle for washing several times to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm.
[0059] Example 3 (1) First, add 15 ml of potassium hydroxide aqueous solution (0.67 M) to 500 ml of dimethyl sulfoxide and mix well; (2) Then, 1 g of the washed aramid fiber was added to the above solution and stirred vigorously for 24 hours to obtain an aramid nanofiber stock solution; (3) Then, the obtained aramid micron fiber slurry solution was further diluted 4 times with ethanol and ultrasonically treated for 30 minutes to obtain the aramid nanofiber slurry; (4) Finally, in order to ensure the uniformity of the thickness of the ultra-thin aramid nanofiber diaphragm, 20 mL of aramid nanofiber slurry was taken and divided into two parts. After the first part of the aramid nanofiber slurry was filtered, the filtration bottle was rotated 180° horizontally, and the second part of the aramid nanofiber slurry was added for filtration. After the filtration was completed, deionized water was added to the filtration bottle for washing several times to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm.
[0060] Example 4 10 mL of the aramid nanofiber slurry in Example 1 was taken, vacuum-assisted filtration, dried, and the filter membrane was removed to obtain the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm.
[0061] Fig.16 a is a digital photo of the aramid nanofiber membrane prepared in Example 4. As can be seen from the figure, the thickness of the aramid nanofiber membrane is 2 μm. Fig.16 b is the cycle curve of the symmetrical battery prepared by using the aramid nanofiber membrane prepared in Example 4. It can be found from the figure that the battery prepared by using the aramid nanofiber membrane has a high cycling rate at 5 mA cm -2 / 2.5mAh cm -2 Under the same conditions, a short circuit occurred after 111 hours of cycling. Reducing the thickness of the aramid nanofiber separator is beneficial to improving the energy density, but too thin a thickness will shorten the cycle life of the battery and be detrimental to the electrochemical long-cycle stability of the battery.
[0062] Industrial applicability: The present invention relates to an ultra-thin, flame-retardant, electrically insulating aramid nanofiber porous diaphragm suitable for large-scale preparation of aqueous zinc ion batteries, which has a nanopore structure, uniform pore size distribution, high porosity, excellent mechanical properties (tensile strength greater than 100MPa), flame retardancy, good electrical insulation performance, large absorption capacity and high absorption rate for aqueous electrolytes, excellent electrochemical and battery performance, and is suitable for aqueous zinc ion batteries. The synthesis method of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber porous diaphragm prepared by the present invention is fast and convenient, has low cost, and is easy to prepare in large quantities. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm provided by the present invention is used for aqueous zinc ion batteries and large-scale energy storage, and has good application prospects.
Claims
1. An ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm, characterized in that: The ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is a layered, porous network structure formed by interweaving and stacking electronegative aramid nanofibers; the diameter of the aramid nanofibers is 1 to 20 nanometers and the length is 1 to 100 microns; the thickness of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane is adjustable, and its thickness is 2 to 20 μm, preferably 5 to 10 μm.
2. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane according to claim 1, characterized in that: The aramid nanofibers in the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane are interwoven to form a nanoscale porous structure with high porosity and excellent mechanical properties; the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane has good hydrophilicity, high adsorption rate for aqueous electrolyte, and excellent electrochemical properties.
3. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane according to claim 1 or 2, characterized in that: In the ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm, the pore size of the porous structure is 100 to 250 nm.
4. The ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane according to any one of claims 1 to 3, characterized in that: The ultra-thin, flame-retardant, electrically insulating aramid nanofiber diaphragm has excellent mechanical properties, with a tensile strength of 110 to 130 MPa and a Young's modulus of 40 to 50 GPa.
5. Use of the ultra-thin, flame-retardant, electrically insulating aramid nanofiber membrane according to any one of claims 1 to 4 in an aqueous zinc ion battery.
Citation Information
Patent Citations
Preparation method and application of large-scale porous aramid fiber microfiber diaphragm
CN111211276A
Polyamide 6 non-woven fabric battery diaphragm for zinc ion battery and preparation method of polyamide 6 non-woven fabric battery diaphragm
CN115275513A
Porous aramid nanofiber film, preparation method thereof and application of porous aramid nanofiber film in battery diaphragm
CN116845478A
Aramid nanofiber / nanocellulose composite zinc ion battery diaphragm, preparation method thereof and zinc ion battery
CN117855747A
Cited By
Aramid nanofiber interface layer modified zinc metal material and application thereof as aqueous zinc ion battery negative electrode material
CN119634202A
Zinc metal materials modified with aramid nanofiber interface layers and their applications as negative electrode materials for aqueous zinc ion batteries
CN119634202B
Preparation method of ultrafine aramid nanofiber dispersion liquid
CN121736320A
Preparation method of superfine aramid nanofiber dispersion liquid
CN121736320B