Organic light-emitting device and display device comprising same

By designing a specific three-layer structure luminescent layer in the stacked OLED device, forming a dopant material concentration gradient, the problem of insufficient luminescence efficiency and life of the stacked OLED device is solved, and higher luminescence efficiency and longer working life are achieved .

CN118973299APending Publication Date: 2024-11-15WUHAN TIANMA MICROELECTRONICS CO LTD SHANGHAI BRANCH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411047499.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Laminated OLED devices have shortcomings in terms of luminous efficiency and life, especially when users have improved their display performance requirements, it is difficult for the prior art to effectively improve their performance.

Method used

An organic light emitting device is designed, including an anode, a cathode and at least two light emitting units arranged between the anode and the cathode, each light emitting unit includes a specific three-layer structure light emitting layer, including a first photon layer and a spacer layer and the second photon layer, the content of the dopant material is high on both sides and the intermediate spacer is low, thereby forming a specific dopant material concentration gradient, reducing exciton quenching, enhancing exciton formation and composite region .

Benefits of technology

It effectively improves the luminous efficiency and working life of organic light emitting devices, significantly extends the service life of the device, and meets the needs of high-performance display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973299A_ABST
    Figure CN118973299A_ABST
Patent Text Reader

Abstract

The invention provides an organic light-emitting device and a display device comprising the same, the organic light-emitting device comprises an anode, a cathode and at least two light-emitting units arranged between the anode and the cathode, and each light-emitting unit independently comprises a light-emitting layer; at least one light-emitting layer comprises a first light-emitting sub-layer, a second light-emitting sub-layer and a spacing layer arranged between the first light-emitting sub-layer and the second light-emitting sub-layer; the mass percentage content of the first doping material in the first light-emitting sub-layer is larger than the mass percentage content of the third doping material in the spacing layer, and the mass percentage content of the second doping material in the second light-emitting sub-layer is larger than the mass percentage content of the third doping material in the spacing layer. The doping material concentration gradient is formed in the at least one light-emitting layer, exciton quenching can be reduced, exciton formation and recombination areas can be enlarged, efficiency roll-off is avoided, the organic light-emitting device has more excellent light-emitting efficiency and stability, and the service life of the device is remarkably prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of display technology, and in particular relates to an organic light-emitting device and a display device comprising the same. Background Art

[0002] Organic Light-Emitting Diode (OLED) is a new generation of display technology that has been popular and has great development prospects in recent years. It has the advantages of self-luminescence, ultra-lightness, wide viewing angle, fast response speed, high luminous efficiency and brightness, wide operating temperature range, simple production process, low power consumption and flexibility. It is currently widely used in many fields such as flat panel displays, flexible displays, automotive displays and solid-state lighting.

[0003] With the continuous development of OLED technology, people gradually found that if a single-layer OLED device wants to achieve high brightness, it will cause a surge in heat due to excessive driving current, thereby reducing the performance and service life of the device. Therefore, achieving high luminous brightness and efficiency at a lower current density and improving the service life of the device are key factors in realizing the industrialization of OLED. The concept of tandem OLED was first proposed by Professor Junji Kido of Yamagata University in Japan in 2003. By connecting at least two single-layer OLED units in series through a charge generation layer, higher luminous brightness and current efficiency can be achieved; at the same time, when measured at the same current density, the aging properties of the tandem OLED and the OLED unit are the same, but due to the high initial brightness of the tandem OLED, when converted to the same initial brightness, the life of the tandem OLED device will be significantly higher than that of the single-layer OLED.

[0004] Although the luminous performance and working life of stacked OLED devices are better than those of single-layer OLED devices, as the application range of the devices increases and users' requirements for display performance increase, the life and luminous efficiency of stacked OLED devices still have obvious shortcomings, and there is a lot of room for performance improvement. Therefore, the field urgently needs to develop stacked OLED devices with higher performance. Summary of the invention

[0005] In order to improve the luminous efficiency and life of a stacked OLED and develop a stacked OLED device with higher luminous performance, one of the objects of the present invention is to provide an organic light-emitting device, which includes an anode, a cathode and at least two light-emitting units arranged between the anode and the cathode, and each of the light-emitting units independently includes a light-emitting layer.

[0006] At least one of the light-emitting layers includes a first light-emitting sublayer, a second light-emitting sublayer and a spacer layer arranged between the first light-emitting sublayer and the second light-emitting sublayer; the first light-emitting sublayer includes a first main material and a first doping material, the second light-emitting sublayer includes a second main material and a second doping material, and the spacer layer includes a third main material and optionally a third doping material.

[0007] The mass percentage of the first doping material in the first luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer, and the mass percentage of the second doping material in the second luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer.

[0008] In the organic light-emitting device provided by the present invention, at least one light-emitting layer adopts a specific three-layer structure design, the first light-emitting sublayer and the second light-emitting sublayer located on both sides have a high content of doping material, and the spacer layer located in the middle has a low content of doping material, so that a specific doping material concentration gradient is formed in the light-emitting layer, which can effectively reduce the quenching of excitons, increase the exciton formation and recombination area, and suppress the efficiency roll-off, so that the organic light-emitting device has higher luminous efficiency and longer service life.

[0009] A second object of the present invention is to provide a display device, which includes the organic light-emitting device as described in the first object.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] In the organic light-emitting device provided by the present invention, at least one light-emitting layer includes a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence, and the content of the doping material in the spacer layer in the middle is lower than the content of the doping material in the first light-emitting sublayer and the second light-emitting sublayer on both sides, so that a specific doping material concentration gradient is formed in the light-emitting layer, which can effectively reduce the quenching of excitons, increase the exciton formation and recombination area, avoid efficiency roll-off, and make the organic light-emitting device have better luminous efficiency and stability, and significantly extend the working life of the device, improve the comprehensive luminous performance, so that it can fully meet the application requirements of stacked OLED devices in high-performance display devices and electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 A schematic diagram of the structure of a light-emitting layer in an organic light-emitting device provided in one embodiment of the present invention;

[0013] Figure 2 A schematic diagram of the structure of an organic light-emitting device provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0014] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0015] In the present invention, the features defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features, and are used to distinguish and describe the features, without distinction of order or importance. In the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.

[0016] In the present invention, the directions or positional relationships indicated by terms such as "upper", "lower", "inside", "outside", "vertical", and "horizontal" are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operated in a specific direction, and should not be understood as limiting the present invention.

[0017] In the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", "installed", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above-mentioned terms in the present invention can be understood according to specific circumstances.

[0018] The present invention has found that a tandem organic electroluminescent device (Tandem OLED) contains at least two light-emitting units connected in series, and adjacent light-emitting units are connected by a charge generation layer (CGL). Compared with a single-layer OLED, a tandem OLED has higher device efficiency and longer lifespan. However, with the increase in the application range of the device and the improvement of user requirements for display performance, existing tandem OLEDs generally have problems of insufficient luminous efficiency and low lifespan. At the same time, the charge generation layer will cause a voltage drop, further reducing the efficiency and lifespan of the tandem device.

[0019] In order to improve the luminous efficiency and life of the stacked OLED and obtain better luminous performance, one embodiment of the present invention provides an organic light-emitting device, which includes an anode, a cathode and at least two light-emitting units arranged between the anode and the cathode, and each of the light-emitting units independently includes a light-emitting layer.

[0020] At least one of the light-emitting layers includes a first light-emitting sublayer, a second light-emitting sublayer and a spacer layer arranged between the first light-emitting sublayer and the second light-emitting sublayer; the first light-emitting sublayer includes a first main material and a first doping material, the second light-emitting sublayer includes a second main material and a second doping material, and the spacer layer includes a third main material and optionally a third doping material.

[0021] The mass percentage of the first doping material in the first luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer, and the mass percentage of the second doping material in the second luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer.

[0022] In the present invention, at least one light-emitting layer has a specific three-layer structure, the first light-emitting sublayer and the second light-emitting sublayer on both sides have a high content of doping material, and the spacer layer in the middle has a low content of doping material (or no doping), so that a specific doping material concentration gradient is formed in the light-emitting layer, which can effectively reduce the quenching of excitons, inhibit efficiency roll-off, increase the exciton formation and recombination area, thereby improving the luminous efficiency and stability of the organic light-emitting device, extending its service life, and giving it better luminescent performance.

[0023] In order to make the above-mentioned purpose, features and effects of the present invention more obvious, the present invention is further described in detail with reference to the accompanying drawings. The accompanying drawings of the present invention are for illustration only and may not be drawn according to the actual scale.

[0024] Figure 1 This is a schematic structural diagram of a light-emitting layer in an organic light-emitting device provided in one embodiment of the present invention, comprising a first light-emitting sublayer 101, a second light-emitting sublayer 102 and a spacer layer 103 arranged between the first light-emitting sublayer 101 and the second light-emitting sublayer 102, the first light-emitting sublayer 101 comprises a first main material and a first doping material, the second light-emitting sublayer 102 comprises a second main material and a second doping material, and the spacer layer 103 comprises a third main material and optionally a third doping material; the mass percentage of the first doping material in the first light-emitting sublayer 101 is greater than the mass percentage of the third doping material in the spacer layer 103, and the mass percentage of the second doping material in the second light-emitting sublayer 102 is greater than the mass percentage of the third doping material in the spacer layer 103.

[0025] It should be noted that the first doping material, the second doping material, and optionally the third doping material in the light-emitting layer can be the same material or different materials; the first main material, the second main material, and the third main material can be the same material or different materials. Based on considerations of preparation processability, material energy level, carrier transport performance, and matching of photoelectric performance, the first doping material, the second doping material, and optionally the third doping material are the same material, and the first main material, the second main material, and the third main material are the same material, so that there is no need to increase the number of chamber evaporation sources in device preparation, thereby reducing preparation costs.

[0026] In some optional embodiments of the present invention, the mass percentage of the first doping material in the first light-emitting sublayer is 0.5-12%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or 11%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0027] And / or, the mass percentage of the second doping material in the second light-emitting sublayer is 0.5-12%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or 11%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0028] And / or, the mass percentage of the third doping material in the spacer layer is ≤3%, for example, it can be 0, 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5% or 2.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0029] In the present invention, "doping material" is also called "guest material", "dye", "luminescent material", which receives energy from the main material and emits a corresponding spectrum to achieve light emission of different colors. According to the luminescence mechanism of the luminescent layer, it can be roughly divided into fluorescent luminescence and phosphorescent luminescence, corresponding to fluorescent doping materials and phosphorescent doping materials respectively; fluorescent doping materials mainly use singlet excitons generated when electrons and holes combine to emit light, and phosphorescent doping materials can use triplet excitons and singlet excitons to emit light at the same time. The present invention optimizes and adjusts the content of doping materials in luminescent layers with different luminescence mechanisms, so that a specific doping material concentration gradient is formed in the luminescent layer, thereby further optimizing the photoelectric performance of the organic light-emitting device and obtaining a higher lifespan and efficiency.

[0030] In some optional embodiments of the present invention, the first doping material, the second doping material and the third doping material are phosphorescent doping materials, and the mass percentage of the first doping material (phosphorescent doping material) in the first light-emitting sublayer is 1-12%, for example, it can be 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or 11%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0031] And / or, the mass percentage of the second doping material (phosphorescent doping material) in the second light-emitting sublayer is 1-12%, for example, it can be 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or 11%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0032] And / or, the mass percentage of the third doping material (phosphorescent doping material) in the spacer layer is ≤3%, for example, it can be 0, 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5% or 2.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0033] In some optional embodiments of the present invention, the first doping material, the second doping material and the third doping material are fluorescent doping materials, and the mass percentage of the first doping material (fluorescent doping material) in the first light-emitting sublayer is 0.5-5%, for example, it can be 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0034] And / or, the mass percentage of the second doping material (fluorescent doping material) in the second light-emitting sublayer is 0.5-5%, for example, it can be 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0035] And / or, the mass percentage of the third doping material (fluorescent doping material) in the spacer layer is ≤2%, for example, it can be 0, 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5% or 1.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0036] In the present invention, for the phosphorescent light-emitting layer, the mass content of the phosphorescent doping material in the spacer layer is preferably ≤3%; for the fluorescent light-emitting layer, the mass content of the fluorescent doping material in the spacer layer is preferably ≤2%, thereby forming a specific doping concentration gradient in the light-emitting layer with high concentration doping on both sides and low concentration doping (or no doping) in the middle, inhibiting exciton quenching and efficiency roll-off, effectively increasing the exciton formation and recombination area, and making the organic light-emitting device have higher luminous efficiency and longer working life. If the content of the doping material in the spacer layer is too high, it will affect the construction of the concentration gradient, and the effect on the effect and life improvement of the device will not be obvious.

[0037] In some optional embodiments of the present invention, the thickness of the first light-emitting sublayer and the second light-emitting sublayer are each independently 8-30nm, for example, 9nm, 10nm, 12nm, 15nm, 18nm, 20nm, 22nm, 25nm or 28nm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0038] And / or, the thickness of the spacer layer is 1-7nm, for example, it can be 1.5nm, 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 4.5nm, 5nm, 5.5nm, 6nm or 6.5nm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and 1-5nm is further preferred.

[0039] The present invention introduces a low doping concentration (or no doping) spacer layer into the light-emitting layer. By further optimizing the thickness of the spacer layer, exciton quenching and efficiency roll-off can be reduced, and while ensuring the luminous brightness, the efficiency and life of the organic light-emitting device can be further improved. If the thickness of the spacer layer is too high, that is, the area with low doping concentration (or no doping) is large, it will affect the luminous brightness of the device and is not conducive to improving the luminous efficiency and life.

[0040] In some optional embodiments of the present invention, the first host material, the second host material and the third host material each independently include any one of an electronic host material, a hole-type host material, a bipolar host material, and an exciplex material, or a combination of at least two thereof.

[0041] Optionally, the first host material, the second host material and the third host material are the same or different, and are further preferably the same, and include but are not limited to any one or a combination of at least two of the following compounds: 4,4'-di(9-carbazole)biphenyl (CBP), 4,4',4"-tri(carbazole-9-yl)triphenylamine (TCTA), 9,9'-diphenyl-9H,9'H-3,3'-bicarbazole (BCzPh), 1,3,5 -tri(carbazol-9-yl)benzene (TCP), 4,4'-bis(carbazol-9-yl)-2,2'-dimethylbiphenyl (CDBP), 3'-(9H-carbazol-9-yl)biphenyl-3,5-dicarbonitrile (mCzB-2CN), 2,2',7,7'-tetra(carbazol-9-yl)-9,9-spirofluorene (spiro-CBP), 4'-(9H-carbazol-9-yl)biphenyl-3,5-dicarbonitrile (PCzB-2CN), 3,6-bis(carbazol-9-yl)-9-(2-ethyl-hexyl)-9H-carbazole (TCz1), bis(2-diphenylphosphine oxide) diphenyl ether (DPEPO), 2,7-bis(9H-carbazol-9-yl)-9,9-dimethylfluorene (DMFL-CBP), 1,3-bis(N-carbazolyl)benzene (mCP), 9-(3-(9H-carbazol-9-yl)phenyl)-9H-carbazole-3-carbonitrile (mCP-C N), 3,3'-di(N-carbazol-9-yl)-1,1'-biphenyl (mCBP), 9-(3-(9H-carbazol-9-yl)phenyl)-3-(diphenylphosphoryl)-9H-carbazole (mCPPO1), 9,9-spirobifluorene-2-yl-diphenylphosphine oxide (SPPO1), 3,5-di(9H-carbazol-9-yl)biphenyl (Ph-mCP), 2-(10-naphthyl-anthracene-9-yl)dibenzofuran.

[0042] In some optional embodiments of the present invention, each of the light-emitting units independently includes a hole transport region and an electron transport region, and the light-emitting layer is disposed between the hole transport region and the electron transport region.

[0043] In some optional embodiments of the present invention, a charge generation layer is disposed between any two adjacent light-emitting units.

[0044] In some optional embodiments of the present invention, a hole injection layer is further provided between the anode and the light-emitting unit adjacent thereto.

[0045] In some optional embodiments of the present invention, an electron injection layer is further provided between the cathode and the light-emitting unit adjacent thereto.

[0046] In some optional embodiments of the present invention, the structural schematic diagram of the organic light-emitting device is as follows Figure 2As shown, it includes an anode 10, a cathode 20, and a first light-emitting unit 30 and a second light-emitting unit 40 disposed between the anode 10 and the cathode 20; a charge generation layer 50 is disposed between the first light-emitting unit 30 and the second light-emitting unit 40; the first light-emitting unit 30 includes a first hole transport region 31, a first electron transport region 33, and a first light-emitting layer 32 disposed between the first hole transport region 31 and the first electron transport region 33; the second light-emitting unit 40 includes a second hole transport region 41, a second electron transport region 43, and a second light-emitting layer 42 disposed between the second hole transport region 41 and the second electron transport region 43. A hole injection layer 60 is disposed between the anode 10 and the first light-emitting unit 30, and an electron injection layer 70 is disposed between the cathode 20 and the second light-emitting unit 40. At least one of the first light-emitting layer 32 and the second light-emitting layer 42 has the structural design of the aforementioned first light-emitting sublayer, the spacer layer, and the second light-emitting sublayer, that is, at least one of the first light-emitting layer 32 and the second light-emitting layer 42 has the following structure: Figure 1 The structure shown.

[0047] In some optional embodiments of the present invention, the hole transport region includes a hole transport layer (HTL) and, optionally, an electron blocking layer (EBL); and / or, the electron transport region includes an electron transport layer (ETL) and, optionally, a hole blocking layer (HBL); and / or, a hole injection layer (HIL) is further provided between the anode and the light-emitting unit adjacent thereto; and / or, an electron injection layer (EIL) is further provided between the cathode and the light-emitting unit adjacent thereto; and / or, a charge generation layer (CGL) is provided between any two adjacent light-emitting units.

[0048] Optionally, the material of the anode can be any one of metal, metal oxide, conductive polymer or a combination of at least two thereof; wherein the metal includes copper, gold, silver, iron, chromium, nickel, manganese, palladium, platinum and alloys thereof; the metal oxide includes indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide, indium gallium zinc oxide (IGZO) and the like; the conductive polymer includes polyaniline, polypyrrole, poly (3-methylthiophene) and the like. In addition to the above materials and combinations thereof that facilitate hole injection, known materials suitable for the anode are also included.

[0049] Optionally, the cathode material may be a metal or a multilayer metal material; wherein the metal includes aluminum, magnesium, silver, indium, tin, titanium, etc. and alloys thereof, and the multilayer metal material includes LiF / Al, LiO2 / Al, BaF2 / Al, etc. In addition to the above materials and combinations thereof that facilitate electron injection, known materials suitable for the cathode are also included.

[0050] It should be noted that the present invention does not particularly limit the materials of the hole injection layer, hole transport region (hole transport layer, optionally electron blocking layer), electron injection layer, and electron transport layer (electron transport layer, optionally hole blocking layer). The hole injection materials, hole transport materials, electron blocking materials, electron injection materials, electron transport materials, and hole blocking materials known in the art can all be applied to the present invention.

[0051] Optionally, the materials of the hole injection layer and the hole transport region (hole transport layer, optionally the electron blocking layer) include but are not limited to any one or a combination of at least two of the following compounds: 4,4',4"-tris(3-methylphenylamino)triphenylamine (MTDATA), 4,4',4"-tris(N,N-diphenyl-amino)triphenylamine (NATA), 4,4',4"-tris(N-(naphthalene-1-yl)-N-phenyl-amino)triphenylamine (1T-NATA), 4,4',4"-tris(N-(naphthalene-2-yl)-N-phenyl-amino)triphenylamine (2TNATA), copper phthalocyanine (CuPc), 1,3,5-tris(4-(diphenylamino)phenyl)benzene (TDAPB), 2,2' -dimethyl-N,N'-di-1-naphthyl-N,N'-diphenyl(1,1'-biphenyl)-4,4'-diamine (α-NPD), 4,4',4"-tri(carbazol-9-yl)triphenylamine (TCTA), 1,3-bis(N-carbazyl)benzene (mCP), 4,4'-di(9-carbazol)biphenyl (CBP), 3,3'-di(N-carbazyl)-1,1'-biphenyl (mCBP), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HATCN), 4,4'-cyclohexylbis(N,N-di(4-methylphenyl)aniline (TAPC), N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl Benzene-4,4'-diamine (α-NPB), N,N'-di(naphthalene-2-yl)-N,N'-di(phenyl)biphenyl-4,4'-diamine (NPB), poly(3,4-ethylenedioxythiophene)-polystyrenesulfonic acid (PEDOT:PSS), 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanoquinodimethane (F4TCNQ), N-(biphenyl-4-yl)-9,9-dimethyl-N-(4-(9-phenyl-9H-carbazole-3-yl)phenyl)-9H-fluorene-2-aminepolyvinylcarbazole (PVK), 4,4'-bis(N-carbazolyl)-1,1'-biphenyl (CBP), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine) (poly -TPD), poly((9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)))(TFB), 1,1-bis(4-(N,N'-di(p-tolyl)amino)phenyl)cyclohexane (TAPC), 3,5-bis(9H-carbazole-9-yl)-N,N-diphenylaniline (DCDPA), N-(biphenyl-4-yl)-9,9-dimethyl-N-(4-(9-phenyl-9H-carbazole-3-yl)phenyl)-9H-fluoren-2-amine, N-(biphenyl-4-yl)-N-(4-(9-phenyl-9H-carbazole-3-yl)phenyl)biphenyl-4-amine, N-((1,1'-biphenyl)-4-yl)-9,9-dimethyl-N-(4-(9-phenyl-9H-carbazole-3-yl)phenyl)-9H-fluorene-2-amine, N4,N4,N4',N4'-tetrakis((1,1'-biphenyl)-4-yl)-(1,1'-biphenyl)-4,4'-diamine)9-phenyl-3,9-bicarbazole (CCP), molybdenum trioxide (MoO3). ,

[0052] Optionally, the materials of the electron injection layer and the electron transport region (electron transport layer, optionally the hole blocking layer) include but are not limited to any one or a combination of at least two of the following compounds: 2,8-bis(diphenylphosphinyl)dibenzothiophene (PPT), diphenyl(4-(triphenylsilyl)phenyl)phosphine oxide (TSPO1), 1,3,5-tri(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), 2,8-bis(diphenylphosphinyl)dibenzofuran (PPF), bis(2-diphenylphosphinyl)diphenyl ether (DPEPO), lithium fluoride (LiF), 4,6-bis(3,5-di(3-pyridyl)phenyl)-2-methylpyrimidine ( B3PYMPM), 4,7-diphenyl-1,10-phenanthroline (Bphen), 1,3,5-tris((3-pyridyl)-3-phenyl)benzene (TmPyBP), 1,3,5-tris(p-pyridin-3-yl-phenyl)benzene (TpPyPB), tris(2,4,6-trimethyl-3-(3-pyridinyl)phenyl)borane (3TPYMB), 1,3-bis(3,5-bipyridin-3-ylphenyl)benzene (B3PYPB), 1,3-bis(3,5-bi(pyridin-3-yl)phenyl)benzene (BMPYPHB), 2,4,6-tris(biphenyl-3-yl)-1,3,5-triazine (T2T), diphenylbis(4-( pyridin-3-yl)phenyl)silane (DPPS), cesium carbonate (Cs2CO3), bis(2-methyl-8-hydroxyquinoline-N1,O8)-(1,1'-biphenyl-4-hydroxy)aluminum (BAlq), 8-hydroxyquinoline-lithium (LiQ), tris(8-hydroxyquinoline)aluminum (Alq3), 2-biphenyl-4-yl-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (PBD), spiro-PBD, 2,9-bis(naphthalene-2-yl)4,7-diphenyl-1,10-phenanthroline (NBphen), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), 3-(4-biphenyl)-4-phenyl-5-tert-butylphenyl Butylphenyl-1,2,4-triazole (TAZ), 4-(naphthalen-1-yl)-3,5-diphenyl-4H-1,2,4-triazole (NTAZ), 2,4,6-tris(3'-(pyridin-3-yl)biphenyl-3-yl)1,3,5-triazine (TmPPPyTz), poly(9,9-bis(3'-(N,N-dimethyl)-N-ethylammonium)-propyl)-2,7-fluorene)-alt-2,7-(9,9-dioctylfluorene))(PFNBr), tris(phenylquinoxaline) (TPQ), 2-(4-(9,10-di-2-naphthalen-2-yl-2-anthracen-2-yl)phenyl)-1-phenyl-1H-benzimidazole (ZADN).

[0053] In some optional embodiments of the present invention, the charge generation layer includes a p-type layer, an n-type layer, and a barrier layer disposed between the p-type layer and the n-type layer.

[0054] In some optional embodiments of the present invention, the p-type layer includes a p-type main material and a p-type dopant, the n-type layer includes an n-type main material and an n-type dopant, and the barrier layer includes a p-type main material and / or an n-type main material.

[0055] Optionally, the p-type main material includes any one or a combination of at least two of aromatic amine compounds.

[0056] Optionally, the p-type dopant includes any one or a combination of at least two of the following groups: cyano, fluorine, chlorine, trifluoromethyl, trifluoromethoxy.

[0057] Optionally, the n-type main material includes any one or a combination of at least two of the following groups: pyridyl, pyrazinyl, pyrimidine, pyridazine, triazine, quinoline, isoquinoline, quinoxaline, quinazoline, benzopyridazine, o-phenanthroline (phenanthroline).

[0058] Optionally, the n-type dopant includes any one of alkali metals, alkali metal compounds, transition metals, and transition metal compounds, or a combination of at least two of them.

[0059] In some optional embodiments of the present invention, the n-type dopant includes any one of Li, Cs, Yb, and Cs2CO3, or a combination of at least two of them.

[0060] Optionally, the material of the barrier layer includes sp 2 Hybridized nitrogen atom groups, such as pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, triazinyl, quinolyl, isoquinolyl, quinoxalinyl, quinazoline, o-phenanthroline (phenanthroline), benzopyridazinyl, etc. The barrier layer can effectively capture the n-type dopant in the n-type layer, confine the n-type dopant in the n-type layer (n-doped), avoid interface deterioration caused by diffusion of the n-type dopant into the p-type layer, reduce the thickness of the depletion layer, and improve the stability of the device.

[0061] In some optional embodiments of the present invention, the LUMO energy level of the barrier layer is 2.5-2.9eV, for example, it can be 2.55eV, 2.6eV, 2.65eV, 2.7eV, 2.75eV, 2.8eV or 2.85eV, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range. The HOMO energy level of the barrier layer is 5.5-6.0eV, for example, it can be 5.55eV, 5.6eV, 5.65eV, 5.7eV, 5.75eV, 5.8eV, 5.85eV, 5.9eV or 5.95eV, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0062] Optionally, the HOMO energy level of the barrier layer is as close as possible to the LUMO energy level of the p-type layer (p-doped), thereby effectively reducing the potential barrier between the charge generation layers, and the mobility is about 10 -4 -10 -3 cm 2 / Vs, the charge generation layer formed with the p-type layer can effectively generate charges, thereby improving the light-emitting performance and service life of the organic light-emitting device of the stacked structure.

[0063] In some optional embodiments of the present invention, the thickness of the p-type layer and the n-type layer are each independently 2-30nm, for example, 3nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm, 20nm, 22nm, 25nm or 28nm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0064] And / or, the thickness of the barrier layer is 0.5-2 nm, for example, it can be 0.6 nm, 0.8 nm, 1 nm, 1.2 nm, 1.5 nm or 1.8 nm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0065] In some optional embodiments of the present invention, each of the light-emitting units is independently selected from any one of a green light-emitting unit, a blue light-emitting unit, a red light-emitting unit or a yellow light-emitting unit.

[0066] As a green light-emitting unit, the green light doping material of its (green) light-emitting layer exemplarily includes but is not limited to any one or a combination of at least two of the following compounds: tris(2-phenylpyridine)iridium(III) (Ir(ppy)3), fac-tris(2-phenylpyridine)iridium(III) (fac-Ir(ppy)3), bis(2-phenylpyridine)(acetylacetonate)iridium(III) (Ir(ppy)2(acac)), tris(2-(p-tolyl)pyridine)iridium(III) (Ir(mppy)3), bis(2-(naphthalene-2-yl)pyridine)(acetylacetonate)iridium(III) (Ir(npy)2(acac)), tris(2-phenyl-3-methyl-pyridine)iridium (Ir(3mppy)3).

[0067] As a blue light-emitting unit, the blue light doping material of its (blue) light-emitting layer exemplarily includes but is not limited to any one of the following compounds or a combination of at least two thereof: perylene, 4,4'-bis(4-(di-p-tolylamino)phenyl)biphenyl (DPAVBi), 4-(di-p-tolylamino)-4,4'-((di-p-tolylamino)phenyl))phenylene (DPAVB), 4,4'-bis(4-(diphenylamino)phenyl)biphenyl (BDAVBi), 2,7-bis(4-diphenylamino)phenyl)biphenyl (DPB), 1,4-bis(2-(4-(N,N-di(p-tolyl)amino)phenyl)vinyl)benzene (DSB), 1,4-bis(N,N-diphenyl)amino)phenylvinylbenzene (DSA), 2,5,8,11-tetra-tert-butylperylene (TBPe), bis(2-hydroxyphenyl)pyrido)beryllium (Bepp2), 9-(9-phenylcarbazol-3-yl)-10-(naphthalene-1-yl)anthracene (PCAN), 1,6-bis(diphenylamino)pyrene.

[0068] As a red light-emitting unit, the red light doping material of its (red) light-emitting layer exemplarily includes but is not limited to any one of the following compounds or a combination of at least two of them: tris(1-phenylisoquinoline)iridium(III)(Ir(piq)3), (bis(2-(4,6-dimethyl)phenylquinoline))(2,2,6,6-tetramethylheptyl-3,5-dionatoic acid)iridium(III), bis(2-(4-n-hexylphenyl)quinoline)(acetylacetonato)iridium(III)(Hex-Ir(phq)2(acac)), tris(2-(4-n-hexylphenyl)quinoline)iridium(III)(Hex-Ir(phq)3), tris(2-phenyl-4-methylquinoline)iridium(III)(Ir(Mphq)3), bis(2-phenylquinoline)(2,2,6,6-tetramethylheptyl-3,5-dionatoic acid)iridium(III)(Ir(dpm)PQ2), bis(phenylisoquinoline)-2,2 ,6,6-tetramethylheptyl-3,5-dionato)iridium(III)(Ir(dpm)(piq)2), bis((4-n-hexylphenyl)isoquinolinato)(acetylacetonato)iridium(III)(Hex-Ir(piq)2(acac)), tris(2-(4-n-hexylphenyl)quinolinato)iridium(III)(Hex-Ir(piq)3), tris(2-(3-methylphenyl)-7-methyl-quinolinato)iridium(Ir(dmp q)3), bis(2-(2-methylphenyl)-7-methyl-quinolyl)(acetylacetonate)iridium(III) (Ir(dmpq)2(acac)), bis(2-(3,5-dimethylphenyl)-4-methyl-quinolyl)(acetylacetonate)iridium(III) (Ir(mphmq)2(acac)), tris(dibenzoylmethane)mono(1,10-phenanthroline)europium(III) (Eu(dbm)3(phen)).

[0069] It should be noted that the number of light-emitting units in the organic light-emitting device is recorded as n, n≥2, for example, it can be 2, 3, 4, 5, 6, etc. Each light-emitting unit includes a light-emitting layer, and each light-emitting unit / light-emitting layer is the same or different. At least one (for example, 1, 2, 3, etc.) of the light-emitting layers has the structural design of the aforementioned first light-emitting sublayer, spacer layer and second light-emitting sublayer. Since the composition of the white light lifetime in the display device is composed of R / G / B, among which the green light lifetime accounts for the highest proportion, accounting for more than 80%, in order to improve the white light lifetime, the improvement of the green light lifetime is particularly important. Based on this, the structural design of the first light-emitting sublayer, spacer layer and second light-emitting sublayer (such as Figure 1 As shown), a specific doping concentration gradient is formed in the green light-emitting layer, which can reduce the efficiency roll-off, increase the exciton formation and recombination area, and thus improve the efficiency and life.

[0070] In some optional embodiments of the present invention, the light-emitting unit is a green light-emitting unit, and the light-emitting layer in the green light-emitting unit includes a first light-emitting sublayer, a second light-emitting sublayer and a spacer layer arranged between the first light-emitting sublayer and the second light-emitting sublayer.

[0071] The first light-emitting sublayer includes a first host material and a first green light doping material, the second light-emitting sublayer includes a second host material and a second green light doping material, and the spacer layer includes a third host material and optionally a third green light doping material.

[0072] The mass percentage of the first green light doping material in the first luminescent sublayer is greater than the mass percentage of the third green light doping material in the spacer layer, and the mass percentage of the second green light doping material in the second luminescent sublayer is greater than the mass percentage of the third green light doping material in the spacer layer.

[0073] In some optional embodiments of the present invention, a light extraction layer (CPL, also known as "covering layer", "cathode covering layer" or "capping layer") is further provided on the side of the cathode away from the light-emitting unit.

[0074] In some optional embodiments of the present invention, the organic light-emitting device can be prepared by the following method: forming an anode on a transparent or opaque smooth substrate, forming various organic thin layers on the anode, and forming a cathode on the organic thin layers. The organic thin layers can be formed by known film-forming methods such as evaporation, sputtering, spin coating, dipping, ion plating, etc.

[0075] An embodiment of the present invention further provides a display device, which includes any one of the organic light-emitting devices provided by the embodiments of the present invention.

[0076] Since the display device adopts the above organic light emitting device, the display device also has the technical effect of the organic light emitting device in the above embodiment. It should be noted that the display device provided by the embodiment of the present invention may also include other circuits and devices for supporting the normal operation of the display device.

[0077] The display device illustratively includes, but is not limited to: any one of a mobile phone, a tablet computer, an electronic photo frame, an electronic paper, and a vehicle-mounted display device.

[0078] Several embodiments of the organic light-emitting device (stacked OLED device) of the present invention are listed below by way of example; the structures of the compounds involved in the following embodiments are as follows:

[0079]

[0080]

[0081] Example 1

[0082] An organic light-emitting device comprises an anode, a cathode and two light-emitting units arranged between the anode and the cathode, and specifically comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a method for preparing the organic light-emitting device comprises the following steps:

[0083] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0084] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0085] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0086] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound CBP as a main material, Btp2Ir(acac) as a doping material, the mass ratio of the main material to the doping material is 99:1, and the thickness of the first light-emitting layer is 45 nm;

[0087] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0088] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0089] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0090] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is BPBPA, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 90:10, and the thickness is 10 nm;

[0091] (9) Vacuum evaporation of BPBPA on the p-type layer as a second hole transport layer with a thickness of 90 nm;

[0092] (10) Vacuum-depositing a second light-emitting layer (total thickness 45 nm) on the second hole transport layer, wherein the main material is CBP and the doping material is Btp2Ir(acac); firstly, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 1% and the thickness is 8 nm; then evaporating CBP (undoped) as a spacer layer on the first light-emitting sublayer, wherein the thickness is 7 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 1% and the thickness is 30 nm;

[0093] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0094] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0095] (13) Vacuum evaporate an Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0096] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0097] Example 2

[0098] An organic light-emitting device comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a preparation method comprises the following steps:

[0099] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0100] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0101] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0102] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound CBP as a main material, Ir(ppy)3 as a doping material, the mass ratio of the main material to the doping material is 94:6, and the thickness of the first light-emitting layer is 30 nm;

[0103] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0104] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0105] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0106] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is NPB, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 90:10, and the thickness is 10 nm;

[0107] (9) Vacuum evaporation of BPBPA on the p-type layer as a second hole transport layer with a thickness of 80 nm;

[0108] (10) Vacuum-depositing a second light-emitting layer (total thickness 30 nm) on the second hole transport layer, wherein the main material is CBP and the doping material is Ir(ppy)3; firstly, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 6% and the thickness is 13 nm; then evaporating CBP as a spacer layer (undoped) on the first light-emitting sublayer, with a thickness of 4 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 6% and the thickness is 13 nm;

[0109] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0110] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0111] (13) Vacuum evaporate an Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0112] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0113] Example 3

[0114] An organic light-emitting device comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a preparation method thereof comprises the following steps:

[0115] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0116] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0117] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0118] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound MADN as a main material and TBP as a doping material, the mass ratio of the main material to the doping material is 99.5:0.5, and the thickness of the first light-emitting layer is 17 nm;

[0119] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0120] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0121] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0122] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is BPBPA, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 90:10, and the thickness is 10 nm;

[0123] (9) vacuum evaporating compound BPBPA on the p-type layer as the second hole transport layer with a thickness of 50 nm;

[0124] (10) Vacuum-depositing a second light-emitting layer (total thickness 17 nm) on the second hole transport layer, wherein the main material is MADN and the doping material is TBP; firstly, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 0.5% and the thickness is 8 nm; then evaporating MADN as a spacer layer (undoped) on the first light-emitting sublayer, wherein the thickness is 1 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 0.5% and the thickness is 8 nm;

[0125] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0126] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0127] (13) Vacuum evaporate an Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0128] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0129] Example 4

[0130] An organic light-emitting device comprises an anode, a cathode and two light-emitting units arranged between the anode and the cathode, and specifically comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a preparation method thereof comprises the following steps:

[0131] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0132] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0133] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0134] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound CBP as a main material, Ir(mppy)3 as a doping material, the mass ratio of the main material to the doping material is 88:12, and the thickness of the first light-emitting layer is 35 nm;

[0135] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0136] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0137] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0138] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is BPBPA, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 90:10, and the thickness is 10 nm;

[0139] (9) Vacuum evaporation of BPBPA on the p-type layer as a second hole transport layer with a thickness of 70 nm;

[0140] (10) Vacuum-depositing a second light-emitting layer (total thickness 35 nm) on the second hole transport layer, wherein the main material is CBP and the doping material is Ir(mppy)3; first, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 12% and the thickness is 15 nm; then evaporating CBP doped with Ir(mppy)3 of 3% by mass on the first light-emitting sublayer as a spacer layer, with a thickness of 5 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 12% and the thickness is 15 nm;

[0141] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0142] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0143] (13) Vacuum evaporate an Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0144] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0145] Example 5

[0146] An organic light-emitting device comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a preparation method thereof comprises the following steps:

[0147] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0148] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0149] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0150] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound CBP as a main material, Ir(mppy)3 as a doping material, the mass ratio of the main material to the doping material is 90:10, and the thickness of the first light-emitting layer is 40 nm;

[0151] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0152] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0153] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0154] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is BPBPA, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 95:5, and the thickness is 10 nm;

[0155] (9) Vacuum evaporation of BPBPA on the p-type layer as a second hole transport layer with a thickness of 60 nm;

[0156] (10) Vacuum-depositing a second light-emitting layer (total thickness 40 nm) on the second hole transport layer, wherein the main material is CBP and the doping material is Ir(mppy)3; firstly, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 10% and the thickness is 17.5 nm; then evaporating a CBP spacer layer (undoped) on the first light-emitting sublayer, wherein the thickness is 5 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 10% and the thickness is 17.5 nm;

[0157] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0158] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0159] (13) Vacuum-depositing a Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0160] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0161] Example 6

[0162] An organic light-emitting device comprises the following structures arranged in sequence: a glass substrate with an ITO anode, a hole injection layer, a first hole transport layer, a first light-emitting layer, a first electron transport layer, a charge generation layer (n-type layer, a barrier layer and a p-type layer), a second hole transport layer, a second light-emitting layer, a second electron transport layer, an electron injection layer, a cathode (silver electrode) and a light extraction layer; wherein the second light-emitting layer comprises a first light-emitting sublayer, a spacer layer and a second light-emitting sublayer arranged in sequence; and a preparation method thereof comprises the following steps:

[0163] (1) The glass substrate with the ITO anode was ultrasonically treated in isopropyl alcohol and deionized water for 30 minutes, and then exposed to ozone for cleaning for 10 minutes, and the glass substrate with the ITO anode obtained by magnetron sputtering was mounted on a vacuum deposition device;

[0164] (2) When the vacuum degree is 2×10 -6 Pa, HATCN was vacuum evaporated on the ITO anode layer with a thickness of 10 nm as a hole injection layer;

[0165] (3) vacuum evaporating the compound BPBPA on the hole injection layer as the first hole transport layer with a thickness of 25 nm;

[0166] (4) vacuum evaporating a first light-emitting layer on the first hole transport layer: using an organic compound MADN as a main material, DSA-Ph as a doping material, the mass ratio of the main material to the doping material is 95:5, and the thickness of the first light-emitting layer is 25 nm;

[0167] (5) vacuum evaporating compound TPBI on the first light-emitting layer as the first electron transport layer with a thickness of 10 nm;

[0168] (6) vacuum evaporating an n-type layer on the first electron transport layer, wherein the n-type main material is BCP, the n-type dopant is Li, the mass ratio of the n-type main material to the n-type dopant is 98:2, and the thickness is 20 nm;

[0169] (7) vacuum evaporating compound BCP on the n-type layer as a barrier layer with a thickness of 1 nm;

[0170] (8) vacuum evaporating a p-type layer on the barrier layer, wherein the p-type main material is BPBPA, the p-type dopant is HATCN, the mass ratio of the p-type main material to the p-type dopant is 90:10, and the thickness is 10 nm;

[0171] (9) Vacuum evaporation of BPBPA on the p-type layer as a second hole transport layer with a thickness of 50 nm;

[0172] (10) Vacuum-depositing a second light-emitting layer (total thickness 25 nm) on the second hole transport layer, wherein the main material is MADN and the doping material is DSA-Ph; first, evaporating to obtain a first light-emitting sublayer, wherein the mass content of the doping material is 5% and the thickness is 11 nm; then evaporating MADN doped with DSA-Ph with a mass content of 2% on the first light-emitting sublayer as a spacer layer with a thickness of 3 nm; then evaporating a second light-emitting sublayer on the spacer layer, wherein the mass content of the doping material is 5% and the thickness is 11 nm;

[0173] (11) vacuum evaporating a compound TPBI on the second light-emitting layer as a second electron transport layer with a thickness of 30 nm;

[0174] (12) vacuum evaporating LiQ on the second electron transport layer as an electron injection layer with a thickness of 1 nm;

[0175] (13) Vacuum-depositing a Ag electrode on the electron injection layer as a cathode with a thickness of 10 nm;

[0176] (14) Compound CPL is vacuum evaporated on the cathode as a light extraction layer with a thickness of 70 nm to obtain the organic light-emitting device.

[0177] Comparative Example 1

[0178] An organic light-emitting device, which differs from Example 1 only in that no spacer layer is provided in the second light-emitting layer, that is, the second light-emitting layer uses CBP as the main material and Btp2Ir(acac) as the doping material, the mass content of the doping material is 1%, and the vapor deposition thickness is 45nm; other layers, thicknesses, materials and preparation methods are the same as those in Example 1.

[0179] Comparative Example 2

[0180] An organic light-emitting device, which differs from Example 2 only in that no spacer layer is provided in the second light-emitting layer, that is, the second light-emitting layer uses CBP as the main material and Ir(ppy)3 as the doping material, the mass content of the doping material is 6%, and the vapor deposition thickness is 30nm; other layers, thicknesses, materials and preparation methods are the same as those in Example 2.

[0181] Comparative Example 3

[0182] An organic light-emitting device, which differs from Example 3 only in that no spacer layer is provided in the second light-emitting layer, that is, the second light-emitting layer uses MADN as the main material and TBP as the doping material, the mass content of the doping material is 0.5%, and the vapor deposition thickness is 17nm; other layers, thicknesses, materials and preparation methods are the same as those in Example 3.

[0183] Performance evaluation of OLED devices:

[0184] The current of the OLED device at different voltages was tested with a Keithley 2365A digital nanovoltmeter, and the current was divided by the luminous area to obtain the current density of the OLED device at different voltages. The brightness and radiant energy flux density of the OLED device at different voltages were tested with a Konicaminolta CS-2000 spectroradiometer. Based on the current density and brightness of the OLED device at different voltages, the current density (10 mA / cm 2 ) operating voltage (V) and current efficiency (cd / A); the lifespan T95 (at 50 mA / cm 2 The test data are shown in Table 1.

[0185] Table 1

[0186] Voltage (V) Current efficiency (cd / A) Lifespan (h) Light Color Example 1 5.7 16.1 81 red Example 2 6.5 33.4 53 Green Light Example 3 7.4 3.6 42 Blu-ray Example 4 7.0 29.2 96 Green Light Example 5 7.5 31.3 88 Green Light Example 6 7.9 11.6 41 Blu-ray Comparative Example 1 6.0 14.4 58 red Comparative Example 2 6.8 30.7 35 Green Light Comparative Example 3 7.6 3.0 34 Blu-ray

[0187] According to the test data in Table 1, in the organic light-emitting device provided by the present invention, the device has a lower operating voltage, higher luminous efficiency and longer life through the special design of the doping concentration gradient in the light-emitting layer.

[0188] Compared with Examples 1-3, the light-emitting layers of Comparative Examples 1-3 use conventional uniform doping concentration, the device life and efficiency are low, the driving voltage is high, and the overall performance is worse than that of Examples 1-3.

[0189] The applicant declares that the present invention uses the above embodiments to illustrate the organic light-emitting device of the present invention and the display device including the same, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An organic light-emitting device, characterized in that: The organic light-emitting device comprises an anode, a cathode and at least two light-emitting units arranged between the anode and the cathode, and each of the light-emitting units independently comprises a light-emitting layer; At least one of the light-emitting layers includes a first light-emitting sublayer, a second light-emitting sublayer, and a spacer layer disposed between the first light-emitting sublayer and the second light-emitting sublayer; The first light-emitting sublayer comprises a first host material and a first dopant material, the second light-emitting sublayer comprises a second host material and a second dopant material, and the spacer layer comprises a third host material and optionally a third dopant material; The mass percentage of the first doping material in the first luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer, and the mass percentage of the second doping material in the second luminescent sublayer is greater than the mass percentage of the third doping material in the spacer layer.

2. The organic light-emitting device according to claim 2, characterized in that: The mass percentage of the first doping material in the first luminescent sublayer is 0.5-12%; and / or the mass percentage of the second doping material in the second luminescent sublayer is 0.5-12%; and / or the mass percentage of the third doping material in the spacer layer is ≤3%.

3. The organic light-emitting device according to claim 2, characterized in that: The first doping material, the second doping material and the third doping material are phosphorescent doping materials, the mass percentage of the first doping material in the first luminescent sublayer is 1-12%; and / or, the mass percentage of the second doping material in the second luminescent sublayer is 1-12%; and / or, the mass percentage of the third doping material in the spacer layer is ≤3%.

4. The organic light-emitting device according to claim 1, characterized in that: The first doping material, the second doping material and the third doping material are fluorescent doping materials, the mass percentage of the first doping material in the first luminescent sublayer is 0.5-5%; and / or, the mass percentage of the second doping material in the second luminescent sublayer is 0.5-5%; and / or, the mass percentage of the third doping material in the spacer layer is ≤2%.

5. The organic light-emitting device according to claim 1, characterized in that: The thickness of the first luminescent sublayer and the second luminescent sublayer are independently 8-30 nm; and / or the thickness of the spacer layer is 1-7 nm.

6. The organic light emitting device according to claim 1, characterized in that: The first host material, the second host material and the third host material each independently include any one of an electron-type host material, a hole-type host material, a bipolar host material and an exciplex material, or a combination of at least two thereof.

7. The organic light-emitting device according to claim 1, characterized in that: Each of the light-emitting units independently comprises a hole transport region and an electron transport region, and the light-emitting layer is arranged between the hole transport region and the electron transport region.

8. The organic light-emitting device according to claim 7, characterized in that: The hole transport region includes a hole transport layer and optionally an electron blocking layer; and / or, the electron transport region comprises an electron transport layer and optionally a hole blocking layer; And / or, a hole injection layer is further provided between the anode and the light-emitting unit adjacent thereto; and / or, an electron injection layer is further provided between the cathode and the light-emitting unit adjacent thereto; And / or, a charge generation layer is disposed between any two adjacent light-emitting units.

9. The organic light emitting device according to claim 8, characterized in that: The charge generation layer includes a p-type layer, an n-type layer, and a barrier layer disposed between the p-type layer and the n-type layer.

10. The organic light emitting device according to claim 9, characterized in that: The p-type layer includes a p-type main material and a p-type dopant, the n-type layer includes an n-type main material and an n-type dopant, and the barrier layer includes a p-type main material and / or an n-type main material.

11. The organic light emitting device according to claim 9, characterized in that: The LUMO energy level of the barrier layer is 2.5-2.9 eV, and the HOMO energy level is 5.5-6.0 eV.

12. The organic light emitting device according to claim 9, characterized in that: The thickness of the p-type layer and the n-type layer are independently 2-30 nm; and / or the thickness of the barrier layer is 0.5-2 nm.

13. The organic light emitting device according to claim 1, characterized in that: Each of the light-emitting units is independently selected from any one of a green light-emitting unit, a blue light-emitting unit, a red light-emitting unit or a yellow light-emitting unit.

14. The organic light emitting device according to claim 1, characterized in that: The light-emitting unit is a green light-emitting unit, and the light-emitting layer in the green light-emitting unit includes a first light-emitting sublayer, a second light-emitting sublayer, and a spacer layer arranged between the first light-emitting sublayer and the second light-emitting sublayer; The first light-emitting sublayer comprises a first host material and a first green light doping material, the second light-emitting sublayer comprises a second host material and a second green light doping material, and the spacer layer comprises a third host material and optionally a third green light doping material; The mass percentage of the first green light doping material in the first luminescent sublayer is greater than the mass percentage of the third green light doping material in the spacer layer, and the mass percentage of the second green light doping material in the second luminescent sublayer is greater than the mass percentage of the third green light doping material in the spacer layer.

15. The organic light emitting device according to claim 1, characterized in that: A light extraction layer is also provided on a side of the cathode away from the light emitting unit.

16. A display device, characterized in that: The display device comprises the organic light-emitting device according to any one of claims 1 to 15.