Perovskite light absorption layer preparation method, perovskite light absorption layer cell, cell preparation method, photovoltaic module and photovoltaic system
By using the three-source co-evaporate method and spin coating method to form the perovskite light absorbing layer in perovskite silicon stacked solar cells, the problem of battery instability caused by the dual-source co-evaporation method is solved, and the photoelectric conversion efficiency of the battery is improved and stability.
Patent Information
- Application Number
- CN202411038729.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
In perovskite silicon stacked solar cells, the use of dual source co-evaporation PbI2 and CsBr to prepare the inorganic frame layer leads to obstacles infiltration of organic salt solutions, leaving more PbI2, resulting in cell instability and current density-voltage characteristics lag.
The three-source co-evaporation method is used to form an inorganic frame layer on the suede substrate, and the organic salt solution is coated using spin coating or slit coating method. RbCl is introduced to expand the crystalline crystal surface spacing and stabilize PbI2 to form a perovskite light absorbing layer. .
The quality and stability of the perovskite film are improved, the reaction ability of the inorganic frame layer and the organic salt solution is enhanced, and the photoelectric conversion efficiency and stability of the battery are improved.
Smart Images

Figure CN118973358A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a method for preparing a perovskite light-absorbing layer and a battery thereof, a battery preparation method, a photovoltaic module, and a photovoltaic system. Background Art
[0002] With the rapid development of perovskite silicon tandem solar cells, their certified power conversion efficiency (PCE) has reached 33.9%.
[0003] In the field of industrial velvet perovskite silicon stacked cells, most use dual-source co-evaporation of PbI2 (lead iodide) and CsBr (cesium bromide) to prepare the inorganic framework layer, and then use the organic salt solution method to prepare the perovskite film on the inorganic framework layer. This preparation method has better efficiency.
[0004] However, the inorganic framework layer prepared by dual-source co-evaporation of PbI2 (lead iodide) and CsBr (cesium bromide) is relatively dense, resulting in penetration barriers for the organic salt solution, which in turn leaves more PbI2 at the bottom of the inorganic framework layer. More PbI2 will lead to instability of the prepared battery device and a larger lag in the current density-voltage (JV) characteristics.
[0005] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0006] The embodiments of the present application provide a method for preparing a perovskite light-absorbing layer and a battery thereof, a battery preparation method, a photovoltaic module, and a photovoltaic system to solve or alleviate one or more of the technical problems raised above.
[0007] A first aspect of an embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising:
[0008] Providing a suede substrate, on which a first compound, a second compound and a third compound are co-evaporated from three sources to form an inorganic framework layer, wherein the first compound is lead iodide, the second compound is cesium iodide, cesium bromide or cesium chloride, and the third compound is rubidium chloride, rubidium iodide or rubidium bromide;
[0009] coating an organic salt solution on the inorganic framework layer by a spin coating method or a slit coating method to obtain a perovskite film;
[0010] The perovskite film is annealed to obtain a perovskite light absorbing layer.
[0011] Optionally, in the perovskite light-absorbing layer, the mass ratio of rubidium is 0.1%-1%;
[0012] And / or, the thickness of the perovskite light absorbing layer is 400-800 nanometers.
[0013] Optionally, the preparation of the suede substrate comprises:
[0014] Provide crystalline silicon bottom cells;
[0015] A tunneling layer and a hole transport layer are sequentially prepared on the crystalline silicon bottom cell to obtain the suede substrate.
[0016] Optionally, the preparation of the crystalline silicon bottom cell includes:
[0017] Providing an N-type silicon wafer substrate with a textured surface, wherein the silicon wafer substrate has a first surface and a second surface opposite to each other;
[0018] Sequentially preparing a first intrinsic amorphous silicon layer and an N-type amorphous silicon layer on the first surface of the silicon wafer substrate;
[0019] A second intrinsic amorphous silicon layer, a P-type amorphous silicon layer, a first conductive layer and a first metal electrode layer are sequentially prepared on the second surface of the silicon wafer substrate.
[0020] Optionally, the first conductive layer is a first transparent conductive oxide layer;
[0021] And / or, the tunneling layer is a second transparent conductive oxide layer.
[0022] Optionally, the thickness of the inorganic framework layer is 300-500 nanometers.
[0023] Optionally, the preparation of the organic salt solution comprises:
[0024] Dissolve formamidine iodine, formamidine bromide and methylamine thiocyanate in isopropyl acetone solvent;
[0025] The isopropyl ketone solvent is stirred until the formamidinium iodine and the formamidinium bromide are completely dissolved to obtain the organic salt solution, wherein the concentration of the formamidinium iodine is within a first preset range, the concentration of the formamidinium bromide is within a second preset range, and the concentration of the methylamine thiocyanate is within a third preset range.
[0026] A second aspect of the present application provides a method for preparing a perovskite crystalline silicon tandem cell, comprising:
[0027] Preparing a perovskite light absorbing layer, wherein the perovskite light absorbing layer is prepared by using the above-mentioned method for preparing a perovskite light absorbing layer;
[0028] An electron transport layer, a second conductive layer and a second metal electrode layer are sequentially prepared on the perovskite light-absorbing layer to obtain a perovskite crystalline silicon stacked cell.
[0029] Optionally, the method further comprises:
[0030] A buffer layer is prepared between the electron transport layer and the second conductive layer.
[0031] Optionally, the method further comprises:
[0032] A buffer modification layer is prepared between the buffer layer and the electron transport layer.
[0033] Optionally, the material of the buffer modification layer is at least one of zinc oxide aluminum, zinc oxide, and tungsten oxide nanoparticles;
[0034] And / or, the thickness of the buffer modification layer is 1-10 nanometers.
[0035] A third aspect of an embodiment of the present application provides a perovskite crystalline silicon stacked cell, comprising: a velvet substrate, and a perovskite light absorbing layer, an electron transport layer, a second conductive layer and a second metal electrode layer stacked in sequence on the velvet substrate, wherein the perovskite light absorbing layer is prepared by the above-mentioned perovskite light absorbing layer preparation method.
[0036] A fourth aspect of an embodiment of the present application provides a photovoltaic module, comprising at least one cell string, wherein the cell string comprises at least two perovskite crystalline silicon stacked cells as described above.
[0037] A fourth aspect of an embodiment of the present application provides a photovoltaic system, comprising the photovoltaic component as described above.
[0038] The above technical solution adopted in the embodiment of the present application may have the following advantages:
[0039] By first using a three-source co-evaporation method to form an inorganic framework layer as a supporting skeleton in the velvet substrate, and then coating the inorganic framework layer with an organic salt solution by spin coating or slit coating, a perovskite film is formed, and finally, the perovskite film is annealed to obtain a perovskite light-absorbing layer. The method for preparing the perovskite light-absorbing layer in this embodiment first uses a three-source co-evaporation method to conformally grow a layer of inorganic framework layer on a micron-sized pyramid on a velvet substrate as a supporting skeleton, so that the subsequent perovskite film formed after the inorganic framework layer is slit-coated with an organic salt solution can be well conformally grown on the micron-sized pyramid. In addition, since the Rb ions in the introduced third compound (such as RbCl) have a large atomic radius, this modification produces an enlarged crystal plane spacing in the inorganic framework layer, which is conducive to the full reaction between the inorganic framework layer and the organic salt solution, thereby improving the quality of the perovskite film. In addition, the introduced third compound (such as RbCl) can form an inactive (PbI2)2RbCl with the residual PbI2 to stabilize the perovskite, which can further improve the stability and quality of the perovskite layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0041] Figure 1 It is a schematic flow chart of the method for preparing a perovskite light-absorbing layer provided in an embodiment of the present application.
[0042] Figure 2 It is a schematic flow chart of the method for preparing the perovskite crystalline silicon tandem battery provided in the embodiment of the present application.
[0043] Figure 3 It is a schematic diagram of the structure of the perovskite crystalline silicon tandem battery provided in the embodiment of the present application.
[0044] Explanation of the accompanying drawings: 1. velvet substrate; 2. perovskite light absorption layer; 3. electron transport layer; 4. second conductive layer; 5. second metal electrode layer; 10. first metal electrode layer; 11. first conductive layer; 12. P-type amorphous silicon layer; 13. back intrinsic amorphous silicon layer; 14. N-type silicon wafer substrate; 15. front intrinsic amorphous silicon layer; 16. N-type amorphous silicon layer; 17. tunneling layer. DETAILED DESCRIPTION
[0045] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0046] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0047] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0048] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0049] To facilitate those skilled in the art to understand the technical solutions provided in the embodiments of the present application, the relevant technologies are described below:
[0050] At present, in the field of industrial velvet perovskite silicon stacked cells, most of them use dual-source co-evaporation of PbI2 and CsBr to prepare the inorganic framework layer. However, the inventors found that the inorganic framework layer prepared by dual-source co-evaporation of PbI2 (lead iodide) and CsBr (cesium bromide) is relatively dense, resulting in penetration barriers of organic salt solutions, which in turn leaves more PbI2 at the bottom of the inorganic framework layer. However, excessive PbI2 is too active and can easily decompose and accelerate ion migration under continuous light, resulting in instability of battery devices and large lag in current density-voltage (JV) characteristics.
[0051] To this end, the embodiment of the present application provides a technical solution for a method for preparing a perovskite light-absorbing layer, which has the following advantages: (1) Rubidium (Rb) ions are introduced. Since Rb ions have a larger atomic radius, this modification produces an enlarged crystal plane spacing in the inorganic framework layer, which is conducive to the full reaction between the inorganic framework layer and the organic salt solution. (2) In view of the problem that unreacted PbI2 leads to poor stability and hysteresis of JV characteristics, the introduced third compound (such as RbCl) forms an inactive (PbI2)2RbCl with the residual PbI2 to stabilize the perovskite, which can improve the stability of the perovskite layer. See below for details.
[0052] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0053] like Figure 1 As shown, an embodiment of the present application provides a method for preparing a perovskite light absorbing layer. The method for preparing a perovskite light absorbing layer may include:
[0054] Step S10, providing a velvet substrate, and three-source co-evaporating a first compound, a second compound, and a third compound on the velvet substrate to form an inorganic framework layer, wherein the first compound is lead iodide (PbI2), the second compound is cesium iodide (CsI2), cesium bromide (CsBr) or cesium chloride (CsCl), and the third compound is rubidium chloride (RbCl), rubidium iodide (RbI) or rubidium bromide (RbBr).
[0055] Step S11, coating an organic salt solution on the inorganic framework layer by spin coating or slit coating to obtain a perovskite film.
[0056] Step S12, annealing the perovskite film to obtain a perovskite light absorbing layer.
[0057] The method for preparing the perovskite light-absorbing layer provided in this embodiment is to form an inorganic framework layer as a supporting skeleton in the velvet substrate by first adopting a three-source co-evaporation method, and then, coating the inorganic framework layer with an organic salt solution by spin coating or slit coating to form a perovskite film, and finally, annealing the perovskite film to obtain the perovskite light-absorbing layer. The method for preparing the perovskite light-absorbing layer in this embodiment is to conformally grow an inorganic framework layer as a supporting skeleton on a micron-sized pyramid on a velvet substrate by first adopting a three-source co-evaporation method, so that the perovskite film formed by the subsequent perovskite film formed after the inorganic framework layer is slit-coated with an organic salt solution can be well conformally grown on the micron-sized pyramid. In addition, since the Rb ions in the introduced third compound (such as RbCl) have a large atomic radius, this modification produces an enlarged crystal interplanar spacing in the inorganic framework layer, which is conducive to the full reaction between the inorganic framework layer and the organic salt solution, thereby improving the quality of the perovskite film. In addition, the introduced third compound (such as RbCl) can form an inactive (PbI2)2RbCl with the residual PbI2 to stabilize the perovskite, which can further improve the stability and quality of the perovskite layer.
[0058] Combine the following Figure 1 , each step in step S10-step S12 and other optional steps are explained in detail.
[0059] Step S10, providing a velvet substrate, and co-evaporating a first compound, a second compound, and a third compound from three sources on the velvet substrate to form an inorganic framework layer, wherein the first compound is lead iodide (PbI2), the second compound is cesium iodide (CsI2), cesium bromide (CsBr) or cesium chloride (CsCl), and the third compound is rubidium chloride (RbCl), rubidium iodide (RbI) or rubidium bromide (RbBr).
[0060] Specifically, the velvet substrate is a layer film with a velvet structure on the surface. In the production and application of solar cells, the irregular surface of the velvet structure can increase the number of reflections of sunlight on the surface, effectively reduce the surface reflectivity of the solar cell, and improve the light absorption coefficient of the device, thereby increasing the photoelectric conversion efficiency of the device. The velvet structure of the velvet substrate described in the present application can also play an effect of reducing light reflection. In this embodiment, the velvet structure is preferably a large velvet structure, for example, a velvet structure with a velvet density of 3-5 microns.
[0061] The second compound is preferably cesium bromide (CsBr).
[0062] The inorganic framework layer is a mixed thin film layer composed of the first compound, the second compound and the third compound, which serves as a supporting skeleton layer to facilitate the subsequent conformal deposition of an organic salt solution thereon. Due to the introduction of Rb ions with a larger atomic radius into the inorganic framework layer, an enlarged crystal interplanar spacing is generated in the formed inorganic framework layer, which is conducive to a full reaction between the inorganic framework layer and the organic salt solution.
[0063] In an optional embodiment, the preparation of the textured substrate includes: providing a crystalline silicon bottom cell; and sequentially preparing a tunneling layer and a hole transport layer on the crystalline silicon bottom cell to obtain the textured substrate.
[0064] Specifically, the crystalline silicon bottom cell is a part of the perovskite crystalline silicon stacked cell, which is composed of crystalline silicon (single crystal silicon or polycrystalline silicon) as the base layer of the perovskite crystalline silicon stacked cell. The main function of the crystalline silicon bottom cell is to absorb photons in the infrared region of the solar spectrum and generate photogenerated charge carriers (electrons and holes).
[0065] The tunneling layer serves as a layer connecting the perovskite top cell and the crystalline silicon bottom cell, allowing electrons to tunnel from one cell layer to another. The tunneling layer can be a thin layer of metal, a layer of transparent conductive oxide or other suitable materials.
[0066] Among them, the tunneling layer can be prepared by magnetron sputtering, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), laser ablation and other methods.
[0067] As an example, an indium tin oxide (ITO) layer may be prepared as the tunneling layer by magnetron sputtering.
[0068] The hole transport layer (HTL) is a key component in the battery structure. Its main function is to transport holes generated by the perovskite light-absorbing layer to the electrode and prevent electrons from passing through, ensuring that the current can flow smoothly and form effective photoelectric conversion.
[0069] The hole transport layer can be prepared by spin coating, slit coating, spray coating and the like.
[0070] The material of the hole transport layer includes but is not limited to one or more of 2PACz (2-phenylacetylimidazole), Me-2PACz (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl phosphate), 4PACz (2-(4-phenylamino)-9H-carbazole-9-yl), Me-4PACz (N,N'-di(4-(3,6-dimethyl-9H-carbazole-9-yl)butyl)-N,N'-dimethyl-4,4'-diaminobenzamide phosphate), and PTAA.
[0071] In this embodiment, the textured substrate is obtained by sequentially preparing a tunneling layer and a hole transport layer on a pre-prepared crystalline silicon bottom cell, thereby shortening the preparation time of the textured substrate.
[0072] In an optional embodiment, the preparation of a crystalline silicon bottom cell includes: providing an N-type silicon wafer substrate with a velvet surface, the silicon wafer substrate having a first side and a second side opposite to each other; sequentially preparing a first intrinsic amorphous silicon layer and an N-type amorphous silicon layer on the first side of the silicon wafer substrate; and sequentially preparing a second intrinsic amorphous silicon layer, a P-type amorphous silicon layer, a first conductive layer and a first metal electrode layer on the second side of the silicon wafer substrate.
[0073] Specifically, the first surface is the front side of the silicon wafer substrate, and the second surface is the back side of the silicon wafer substrate.
[0074] Intrinsic amorphous silicon (ia-Si) is a non-crystalline silicon material that has no intentionally added dopants and is therefore neither a p-type nor an n-type semiconductor. The conductivity of intrinsic amorphous silicon is relatively low because it does not contain additional free carriers (electrons or holes).
[0075] In this embodiment, the intrinsic amorphous silicon layer can be prepared by using PECVD (plasma enhanced chemical vapor deposition) equipment.
[0076] In a specific embodiment, the intrinsic amorphous silicon layer can be prepared by:
[0077] First, the n-type silicon wafer substrate is cleaned to remove contaminants and damaged layers on the surface.
[0078] Afterwards, a PECVD device is used to deposit a layer of intrinsic amorphous silicon film on the front and / or back of the n-type silicon wafer substrate. This preparation process is usually carried out in a mixed atmosphere of silicon-containing gas (such as silane SiH4) and hydrogen. The plasma excites the gas molecules to promote the deposition of silicon atoms on the surface of the silicon wafer to form a film.
[0079] During the deposition process, high concentrations of hydrogen are introduced, which helps passivate dangling bonds on the surface of the silicon wafer, reduce defect density, and improve the quality of the film.
[0080] After the first intrinsic amorphous silicon layer is deposited, an N-type dopant, such as phosphine (PH3), may be introduced and doped during the PECVD process to form an N-type amorphous silicon layer.
[0081] After the second intrinsic amorphous silicon layer is deposited, an N-type dopant may be introduced, and a p-type dopant, such as borane (B2H6), may be introduced and doped during the PECVD process to form a p-type amorphous silicon layer.
[0082] In other embodiments, RF sputtering may be used to form the first intrinsic amorphous silicon layer and the N-type amorphous silicon layer, and to form the second intrinsic amorphous silicon layer and the P-type amorphous silicon layer.
[0083] In the process of preparing the first intrinsic amorphous silicon layer and the N-type amorphous silicon layer by RF sputtering, the silicon target is excited by the RF electric field, and silicon atoms are sputtered onto the substrate to form a thin film. Afterwards, the N-type amorphous silicon layer is prepared by introducing N-type dopant gas during the RF sputtering process.
[0084] In the process of preparing the second intrinsic amorphous silicon layer and the P-type amorphous silicon layer by RF sputtering, the silicon target is excited by the RF electric field, and silicon atoms are sputtered onto the substrate to form a thin film. Afterwards, the P-type amorphous silicon layer is prepared by introducing P-type dopant gas during the RF sputtering process.
[0085] The first conductive layer is mainly used for collecting charges and transmitting current.
[0086] The material of the first conductive layer may be a transparent conductive oxide.
[0087] The first conductive layer can be prepared by magnetron sputtering, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), laser ablation, or the like.
[0088] As an example, an indium tin oxide (ITO) layer may be prepared by a magnetron sputtering method as the first conductive layer.
[0089] The first metal electrode layer serves as the back electrode of the battery and is mainly used to send the generated current to an external circuit to form usable electrical energy.
[0090] The first metal electrode layer can be prepared by thermal evaporation, screen printing and other methods.
[0091] The material of the first metal electrode layer includes, but is not limited to, gold (Au), silver (Ag), aluminum (Al), and copper (Cu).
[0092] As an example, a Ag metal gate line layer may be prepared by thermal evaporation as the first metal electrode layer.
[0093] It should be noted that in other embodiments, the silicon wafer substrate may also be a P-type silicon wafer substrate. When the silicon wafer substrate is a P-type silicon wafer substrate, the preparation method of the crystalline silicon bottom cell is similar to the preparation method when the silicon wafer substrate is an N-type silicon wafer substrate, and will not be repeated in this embodiment.
[0094] In this embodiment, the crystalline silicon bottom cell is made by using an N-type silicon wafer substrate, which is equivalent to using a P-type silicon wafer substrate to make a crystalline silicon bottom cell, and has better conversion efficiency, stability and environmental friendliness.
[0095] In an optional embodiment, the first conductive layer is a first transparent conductive oxide layer; and / or
[0096] The tunneling layer is a second transparent conductive oxide (TCO) layer.
[0097] In this embodiment, the overall performance and stability of the battery can be improved by using the first transparent conductive oxide layer as the first conductive layer. The second transparent conductive oxide (TCO) layer can help improve the open circuit voltage and fill factor of the battery, thereby improving the overall photoelectric conversion efficiency of the battery.
[0098] In an optional embodiment, the material of the first transparent conductive oxide layer and the second transparent conductive oxide layer is at least one of indium tin oxide, indium zinc oxide, aluminum zinc oxide and indium antimony oxide.
[0099] In this embodiment, by using indium tin oxide, indium zinc oxide, zinc aluminum oxide and indium antimony oxide as the material of the transparent conductive oxide layer, the transparent conductive oxide layer can provide higher transparency in the visible light range, thereby improving the conversion efficiency of the battery.
[0100] In an optional embodiment, the thickness of the silicon wafer substrate is 2-5 microns, including any value within the thickness range, for example, 2 microns, 4 microns, and 5 microns.
[0101] In this embodiment, the velvet degree of the silicon wafer substrate is set to a large velvet surface of 2-5 microns, thereby reducing the production cost of the velvet surface.
[0102] In an optional embodiment, the total thickness of the first intrinsic amorphous silicon layer and the N-type amorphous silicon layer is 30-40 nanometers, including any value within the thickness range, for example, 30 nanometers, 35 nanometers, and 40 nanometers.
[0103] In this embodiment, by setting the total thickness of the first intrinsic amorphous silicon layer and the N-type amorphous silicon layer to 30-40 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0104] In an optional embodiment, the total thickness of the second intrinsic amorphous silicon layer and the P-type amorphous silicon layer is 25-35 nanometers, including any value within the thickness range, for example, 25 nanometers, 30 nanometers, and 35 nanometers.
[0105] In this embodiment, by setting the total thickness of the second intrinsic amorphous silicon layer and the P-type amorphous silicon layer to 25-35 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0106] In an optional embodiment, the thickness of the first transparent conductive oxide layer is 80-130 nanometers, including any value within the thickness range, for example, 80 nanometers, 100 nanometers, and 130 nanometers.
[0107] In this embodiment, by setting the thickness of the first transparent conductive oxide layer to 80-130 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0108] In an optional embodiment, the second transparent conductive oxide layer has a thickness of 10-30 nanometers, including any value within the thickness range, for example, 10 nanometers, 20 nanometers, and 30 nanometers.
[0109] In this embodiment, by setting the thickness of the second transparent conductive oxide layer to 10-30 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0110] In an optional embodiment, the thickness of the inorganic framework layer is 300-500 nanometers, including any value within the thickness range, for example, 300 nanometers, 400 nanometers, and 500 nanometers.
[0111] In this embodiment, by setting the thickness of the inorganic framework layer to 300-500 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0112] In an optional embodiment, preparing a hole transport layer on the crystalline silicon bottom cell includes: preparing the hole transport layer on the tunneling layer by a slit coating method.
[0113] In this embodiment, the hole transport layer is prepared on the tunnel layer by using a slit coating method, so that the slit coating equipment for coating the organic salt solution can be reused to prepare the hole transport layer without using other equipment to prepare the hole transport layer, thereby saving costs.
[0114] In an optional embodiment, the hole transport layer has a thickness of 1-10 nanometers, including any value within the thickness range, for example, 1 nanometer, 5 nanometers, and 10 nanometers.
[0115] In this embodiment, by setting the thickness of the hole transport layer to 1-10 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0116] Step S11, coating an organic salt solution on the inorganic framework layer by spin coating or slit coating to obtain a perovskite film.
[0117] Specifically, after the inorganic framework layer is prepared, an organic salt solution may be coated on the inorganic framework layer by a spin coating method or a slit coating method to obtain a perovskite film.
[0118] The organic salt solution is a precursor solution for preparing a perovskite film.
[0119] As an example, when the organic salt solution is coated on the inorganic framework layer by spin coating, in order to obtain a better coating effect, the spin coating speed can be set to 4000 rpm (Revolutions Per Minute) and the spin coating time can be set to 60 seconds.
[0120] As an example, when the organic salt solution is coated on the inorganic framework layer by a slit coating method, the perovskite film can be obtained by coating in the following manner.
[0121] First, the velvet substrate containing the inorganic framework layer is placed on the sample table of the slit coating equipment, and after the front accompanying film is placed at the front end of the velvet substrate containing the inorganic framework layer, the prepared organic salt solution can be poured into the slit coating blade of the slit coating equipment. Finally, the slit coating blade can be controlled to use the slit coating method to pre-coat from the front accompanying film until the velvet substrate containing the inorganic framework layer is coated to obtain a perovskite film. In addition, during the coating process, the organic salt solution is dried by a wind knife, so that the solvent in the organic salt solution evaporates quickly, thereby accelerating the drying process of the perovskite film and improving the uniformity of the perovskite film. Among them, in order to obtain a better drying effect, the air pressure in the wind knife is preferably controlled within 0.1-0.5Pa.
[0122] In an optional embodiment, the preparation of the organic salt solution includes: dissolving formamidinium iodine (FAI), formamidinium bromide (FABr) and methylammonium thiocyanate (MASCN) in an isopropyl acetone (IPA) solvent; stirring the isopropyl acetone solvent until the formamidinium iodine, the formamidinium bromide and the methylammonium thiocyanate are completely dissolved to obtain the organic salt solution, wherein the concentration of the formamidinium iodine is within a first preset range, the concentration of the formamidinium bromide is within a second preset range, and the concentration of the methylammonium thiocyanate is within a third preset range.
[0123] Specifically, the first preset range, the second preset range and the third preset range can be set according to actual conditions, and their specific values are not limited in this embodiment.
[0124] In a preferred embodiment, the concentration of formamidinium iodine (FAI) is 1200 mg / ml, the concentration of formamidinium bromide (FABr) is 800 mg / ml, and the concentration of methylamine thiocyanate (MASCN) is 119.8 mg / ml.
[0125] In other embodiments, the organic salt solution may be prepared by dissolving at least one other organic salt in an organic solvent.
[0126] Among them, the organic salt can be formamidine iodine (FAI), formamidine bromide (FABr), formamidine chloride (FACl), formamidine thiocyanate (FASCN), formamidine acetate (FACH3COO), methylamine iodine (MAI), methylamine bromide (MABr), methylamine chloride (MACl), methylamine acetate (MACH3COO), methylamine thiocyanate (MASCN), etc.
[0127] The organic solvent may be dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethanol (Ethanol), isopropyl ketone (IPA), ethyl acetate (Ethyl acetate) and the like.
[0128] As an example, methylamine iodine (MAI) and methylamine bromide (MABr) can be dissolved in an ethanol solvent to prepare the organic salt solution. Methylamine iodine (MAI), methylamine bromide (MABr) and methylamine thiocyanate (MASCN) can be dissolved in an isopropyl ketone solvent to prepare the organic salt solution.
[0129] In an optional embodiment, in order to improve the quality and stability of the prepared perovskite light absorbing layer, the mass ratio of rubidium in the perovskite light absorbing layer is 0.1%-1%, including any point value within the mass ratio range, for example, 0.1%, 0.2%, 0.5%, 0.7%, and 1%.
[0130] And / or, in the perovskite light absorbing layer, the particle size of the perovskite is 1-2 microns, including any point value within the particle size range, for example, 1 micron, 1.5, 2 microns.
[0131] And / or, the thickness of the perovskite light absorbing layer is 400-800 nanometers, including any value within the thickness range, for example, 400 nanometers, 500 nanometers, 600 nanometers, 700 nanometers, and 800 nanometers.
[0132] Step S12, annealing the perovskite film to obtain a perovskite light absorbing layer.
[0133] Specifically, after obtaining the perovskite film, the perovskite film will be annealed so that a more stable and uniform perovskite light-absorbing layer can be formed.
[0134] In an optional embodiment, the band gap of the perovskite layer is 1.63eV-1.70eV.
[0135] In an optional embodiment, the step of annealing the perovskite film to obtain the perovskite light absorbing layer comprises: performing a first annealing treatment on the perovskite film, and after completing the first annealing treatment, performing a second annealing treatment again to obtain the perovskite light absorbing layer.
[0136] Specifically, by performing a first annealing treatment on the perovskite film, a perovskite crystal structure is initially formed, and solvents and other volatile substances are removed to reduce stress and defects in the perovskite film. Thereafter, the perovskite film is subjected to a second annealing treatment to further enhance the orderliness and integrity of the crystal, reduce crystal defects and grain boundaries, and improve the performance and stability of the perovskite light-absorbing layer.
[0137] It should be noted that the first annealing treatment and the second annealing treatment can be performed on one hot stage or on two hot stages.
[0138] In this embodiment, the perovskite film is subjected to two annealing treatments, so that the energy band structure of the perovskite material can be adjusted and the performance and stability of the perovskite film can be improved.
[0139] In an optional embodiment, the annealing temperature of the first annealing treatment is 70-100° C., including any value within the temperature range, such as 70° C., 80° C., 90° C., and 100° C. The annealing time is 2-30 min, including any value within the time range, such as 2 min, 5 min, 10 min, 20 min, 25 min, and 30 min.
[0140] The annealing temperature of the second annealing treatment is 140-160° C., including any value within the temperature range, such as 140° C., 145° C., 150° C., and 160° C. The annealing time is 20-30 min, including any value within the time range, such as 20 min, 25 min, and 30 min.
[0141] In this embodiment, by setting the annealing temperature of the first annealing treatment to 70-100°C and the annealing time to 2-30 minutes, and setting the annealing temperature of the second annealing treatment to 140-160°C and the annealing time to 20-30 minutes, a more stable and uniform perovskite light absorbing layer can be obtained.
[0142] In an optional embodiment, in order to obtain a more stable and uniform inorganic framework layer, after forming the inorganic framework layer, the method further includes: performing annealing treatment on the inorganic framework layer.
[0143] In this embodiment, after the inorganic framework layer is formed, the inorganic framework layer is annealed, so that a more stable and uniform inorganic framework layer can be prepared.
[0144] In an optional embodiment, when the inorganic framework layer is annealed, the annealing temperature is 100-150°C, including any point in this temperature range, for example, 100°C, 120°C, 130°C, 150°C, and the annealing time is 1-5min, including any point in this time range, for example, 1min, 3min, 5min.
[0145] In this embodiment, by setting the annealing temperature of the inorganic framework layer to 100-150° C. and the annealing time to 1-5 min, a more stable and uniform inorganic framework layer can be obtained.
[0146] like Figure 2 As shown, the embodiment of the present application provides a method for preparing a perovskite crystalline silicon tandem battery. The method for preparing a perovskite crystalline silicon tandem battery may include:
[0147] Step S20, preparing a perovskite light absorbing layer, wherein the perovskite light absorbing layer is prepared by using the above-mentioned method for preparing a perovskite light absorbing layer.
[0148] Specifically, the method for preparing the perovskite light absorbing layer has been described in detail in the above embodiments, and will not be repeated in this embodiment.
[0149] Step S21, sequentially preparing an electron transport layer, a second conductive layer and a second metal electrode layer on the perovskite light-absorbing layer to obtain a perovskite crystalline silicon stacked cell.
[0150] Specifically, the electron transport layer (ETL) mainly functions to transport electrons generated by the perovskite light absorption layer and inhibit electron backflow. The electron transport layer is usually composed of materials with good electronic conductivity and chemical stability. The materials of the electron transport layer include one or more of tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C61 butyric acid methyl ester (PC61BM), fullerene (C60), and PDADI.
[0151] The electron transport layer can be prepared by thermal evaporation, solution coating, atomic layer deposition (ALD), chemical vapor deposition (CVD), spin coating, etc.
[0152] As an example, a PDADI layer and a C60 layer as an electron transport layer may be sequentially prepared on the perovskite light absorbing layer by a thermal evaporation method.
[0153] The second conductive layer (Transparent Conductive Layer, TCL) is mainly used for charge transmission and conduction. As an electrode in the battery, it can effectively collect and transport the generated charge and help the battery output current. The second conductive layer is usually composed of indium zinc oxide (IZO) or other transparent conductive oxide materials, which have excellent conductivity and ensure effective collection of current.
[0154] The second conductive layer can be prepared by magnetron sputtering, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), laser ablation and the like.
[0155] The material of the second conductive layer includes, but is not limited to, indium tin oxide (ITO), indium zinc oxide (IZO), aluminum zinc oxide (AZO), and indium antimony oxide (IAO).
[0156] As an example, an indium zinc oxide (IZO) layer may be prepared as the second conductive layer by magnetron sputtering.
[0157] The second metal electrode layer serves as the front electrode of the battery and is mainly used to send the generated current to an external circuit to form usable electrical energy.
[0158] The second metal electrode layer can be prepared by thermal evaporation, screen printing and other methods.
[0159] The material of the second metal electrode layer includes, but is not limited to, gold (Au), silver (Ag), aluminum (Al), and copper (Cu).
[0160] As an example, a Ag metal gate line layer may be prepared by thermal evaporation as the second metal electrode layer.
[0161] In this embodiment, an electron transport layer, a second conductive layer and a second metal electrode layer are sequentially prepared on a more uniform perovskite light absorbing layer to obtain a perovskite crystalline silicon tandem battery, so that the prepared perovskite crystalline silicon tandem battery has better performance.
[0162] In an optional embodiment, the electron transport layer includes a PDADI layer and a C60 layer, and preparing the electron transport layer on the perovskite light absorbing layer includes: preparing the PDADI layer on the perovskite light absorbing layer by spin coating; and preparing the C60 layer on the PDADI layer by thermal evaporation.
[0163] Specifically, the PDADI (1,3-diaminopropane dihydroiodide) layer has excellent electron transport capability, which can effectively extract electrons from the perovskite layer and transfer them to the electrode, thereby improving the current output of the battery. The PDADI layer can also serve as an interface passivation layer, reducing interface defects between the perovskite layer and the electrode, reducing charge recombination, and improving the open circuit voltage (VOC) of the battery.
[0164] As an electron transport material, the C60 (fullerene) layer can efficiently extract electrons from the perovskite layer, reduce the recombination of electrons at the interface, and improve the photoelectric conversion efficiency of the battery.
[0165] In this embodiment, by using the PDADI layer and the C60 layer as electron transport layers, preparing the PDADI layer by spin coating and preparing the C60 layer by thermal evaporation, a stable electron transport layer can be prepared, thereby improving the performance and stability of the battery.
[0166] In an optional embodiment, the thickness of the PDADI layer is 1-5 nanometers, including any value within this thickness range, for example, 1 nanometer, 3 nanometers, and 5 nanometers.
[0167] In this embodiment, by setting the thickness of the PDADI layer to 1-5 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0168] In an optional embodiment, the thickness of the C60 layer is 10-20 nanometers, including any value within this thickness range, for example, 10 nanometers, 15 nanometers, and 20 nanometers.
[0169] In this embodiment, by setting the thickness of the C60 layer to 10-20 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0170] In an optional embodiment, in order to optimize charge transport, improve interface performance, resist sputtering damage, and improve the performance and stability of the solar cell, the method further includes: preparing a buffer layer between the electron transport layer and the second conductive layer.
[0171] Specifically, the buffer layer can be prepared by solution coating, atomic layer deposition (ALD), chemical vapor deposition (CVD) and the like.
[0172] The material of the buffer layer may be one or more of tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C61, methyl butyrate (PC61BM), and the like.
[0173] The material of the buffer layer is preferably tin dioxide (SnO2).
[0174] As an example, a tin dioxide (SnO 2 ) layer may be prepared by atomic layer deposition (ALD) as the buffer layer.
[0175] In an optional embodiment, the buffer layer has a thickness of 10-20 nanometers, including any value within the thickness range, for example, 10 nanometers, 15 nanometers, and 20 nanometers.
[0176] In this embodiment, by setting the thickness of the buffer layer to 10-20 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0177] In an optional embodiment, in order to improve the interface characteristics of the battery, increase the transfer efficiency of charge carriers, and enhance the stability of the battery, the method further includes: preparing a buffer modification layer between the buffer layer and the electron transport layer.
[0178] Specifically, the buffer modification layer can be prepared by solution coating, atomic layer deposition (ALD), chemical vapor deposition (CVD) and the like.
[0179] The material of the buffer modification layer may be one or more of zinc oxide aluminum (AZO), zinc oxide (ZnO), and tungsten oxide (WO3) nanoparticles.
[0180] As an example, the buffer modification layer may be prepared by using an alcohol solution of one or more of zinc aluminum oxide (AZO), zinc oxide (ZnO), and tungsten oxide (WO 3 ) nanoparticles.
[0181] In an optional embodiment, the buffer modification layer has a thickness of 1-10 nanometers, including any value within the thickness range, for example, 1 nanometer, 5 nanometers, 7 nanometers, and 10 nanometers.
[0182] In an optional embodiment, in order to reduce the reflection of light on the surface of the battery, increase the transmittance of light, and improve the battery's light absorption efficiency, the method also includes: preparing an anti-reflection layer on the second metal electrode layer to obtain the perovskite crystalline silicon stacked battery.
[0183] Specifically, the anti-reflection layer can be prepared by a physical vapor deposition (PVD) method, a chemical vapor deposition (CVD) method, a solution method, an atomic layer deposition (ALD) method, an electrochemical deposition method, or the like.
[0184] The material of the anti-reflection layer includes, but is not limited to, magnesium fluoride (MgFx), lithium fluoride (LiF), sodium fluoride (NaF), silicon oxide (SiO2), and PDMS (polydimethylsiloxane).
[0185] In an optional embodiment, the thickness of the second conductive layer is 30-100 nanometers, including any value within the thickness range, for example, 30 nanometers, 50 nanometers, 70 nanometers, and 100 nanometers.
[0186] In this embodiment, by setting the second conductive layer to 30-100 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0187] In an optional embodiment, the thickness of the second metal electrode layer is 200-600 nanometers, including any value within the thickness range, for example, 200 nanometers, 300 nanometers, 400 nanometers, 500 nanometers, and 600 nanometers.
[0188] In this embodiment, by setting the second metal electrode layer to 200-600 nanometers, the cost of raw materials can be saved while satisfying the photoelectric conversion efficiency of the battery.
[0189] like Figure 3 As shown, an embodiment of the present application also provides a perovskite crystalline silicon stacked cell, which includes a velvet substrate 1, and a perovskite light absorption layer 2, an electron transport layer 3, a second conductive layer 4 and a second metal electrode layer 5 stacked in sequence on the velvet substrate 1.
[0190] The perovskite light absorbing layer 2 is prepared by using the perovskite light absorbing layer preparation method described in the above embodiment.
[0191] The preparation methods and materials of the velvet substrate 1 , the electron transport layer 3 , the second conductive layer 4 and the second metal electrode layer 5 have been described in detail in the above embodiments and will not be described in detail in this embodiment.
[0192] In this embodiment, since the perovskite light absorption layer in the perovskite crystalline silicon tandem cell has a higher uniformity, the perovskite crystalline silicon tandem cell has better performance.
[0193] In an optional embodiment, the electron transport layer includes a PDADI layer and a C60 layer.
[0194] In this embodiment, the PDADI layer and the C60 layer are used as electron transport layers, thereby improving the performance and stability of the battery.
[0195] In an optional embodiment, a buffer layer is further included between the electron transport layer 3 and the second conductive layer 4 .
[0196] In this embodiment, a buffer layer is provided between the electron transport layer 3 and the second conductive layer 4 to optimize charge transport, improve interface performance, and thus improve the performance and stability of the solar cell.
[0197] In an optional embodiment, a buffer modification layer is further included between the buffer layer and the electron transport layer 3 .
[0198] In this embodiment, a buffer modification layer is provided between the buffer layer and the electron transport layer 3, thereby improving the interface characteristics of the battery, increasing the transfer efficiency of charge carriers, and enhancing the stability of the battery.
[0199] In an optional embodiment, the second metal electrode layer further includes an anti-reflection layer.
[0200] In this embodiment, an anti-reflection layer is provided on the second metal electrode layer, thereby reducing the reflection of light on the surface of the battery, increasing the light transmittance, and improving the light absorption efficiency of the battery.
[0201] In an optional embodiment, the velvet base 1 includes a first metal electrode layer 10, a first conductive layer 11, a P-type amorphous silicon layer 12, a back intrinsic amorphous silicon layer 13 (the second intrinsic amorphous silicon layer described above), an N-type silicon wafer substrate 14, a front intrinsic amorphous silicon layer 15 (the first intrinsic amorphous silicon layer described above), an N-type amorphous silicon layer 16 and a tunneling layer 17 stacked in sequence.
[0202] Specifically, the preparation methods and materials of the first metal electrode layer 10, the first conductive layer 11, the P-type amorphous silicon layer 12, the back intrinsic amorphous silicon layer 13 (the second intrinsic amorphous silicon layer described above), the N-type silicon wafer substrate 14, the front intrinsic amorphous silicon layer 15 (the first intrinsic amorphous silicon layer described above), the N-type amorphous silicon layer 16 and the tunneling layer 17 have been described in detail in the above embodiments and will not be repeated in this embodiment.
[0203] In this embodiment, the crystalline silicon bottom cell is made by using an N-type silicon wafer substrate, which is equivalent to using a P-type silicon wafer substrate to make a crystalline silicon bottom cell. The perovskite crystalline silicon stacked cell in this embodiment has better conversion efficiency, stability and environmental friendliness.
[0204] The following will conduct performance tests on the perovskite crystalline silicon tandem cells prepared by the preparation methods of the perovskite crystalline silicon tandem cells provided in the following embodiments and the perovskite crystalline silicon tandem cells of the relevant comparative examples, wherein the performance tests include the open circuit voltage Voc, short circuit current density Jsc, fill factor FF, and photoelectric conversion efficiency PCE of the battery device.
[0205] [Example 1]
[0206] A method for preparing a perovskite crystalline silicon stacked cell The specific preparation process is as follows:
[0207] Step 1: Provide an N-type silicon wafer substrate with a thickness of 3 microns.
[0208] Step 2: Use PECVD method to sequentially prepare the first intrinsic amorphous silicon layer and N-type amorphous silicon on the front side of the N-type silicon wafer substrate. The thickness of these two layers is 35 nanometers in total.
[0209] Step 3: A second intrinsic amorphous silicon layer and a P-type amorphous silicon layer are sequentially prepared on the back side of the N-type silicon wafer substrate using the PECVD method. The thickness of the two layers is 30 nanometers in total.
[0210] Step 4: Prepare a front transparent conductive oxide (ITO) layer as a tunneling layer using magnetron sputtering with a thickness of 20 nanometers.
[0211] Step 5: A back transparent conductive oxide (ITO) layer is prepared as the first conductive layer by magnetron sputtering, with a thickness of 120 nanometers.
[0212] Step 6: Deposit a hybrid SAM hole transport layer on the front ITO layer using spin coating with a thickness of 5 nm.
[0213] Step 7: PbI2, CsBr, and RbCl are evaporated on the hole transport layer using a three-source co-evaporation method to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0214] Step 8: The inorganic framework layer is fully reacted with the organic salt solution composed of FAI, FABr and MASCN by spin coating to obtain a perovskite film, and the perovskite light absorbing layer is obtained after annealing, wherein the mass ratio of rubidium in the perovskite light absorbing layer is 0.5%, and the thickness of the perovskite light absorbing layer is 700 nanometers.
[0215] Step 9: Deposit a PDADI layer with a thickness of 2 nm on the perovskite light absorbing layer by spin coating.
[0216] Step 10: Prepare a C60 layer on the PDADI layer using thermal evaporation with a thickness of 15 nm.
[0217] Step 11: A tin dioxide (SnO2) layer is prepared on the C60 layer as a buffer layer by atomic layer deposition, with a thickness of 15 nanometers.
[0218] Step 12: Prepare an indium zinc oxide (IZO) layer as the second conductive layer by magnetron sputtering, with a thickness of 70 nanometers.
[0219] Step 13: Use thermal evaporation to prepare the back and front Ag metal grid line layers as the first metal electrode layer and the second metal electrode layer respectively, with a thickness of 500 nanometers, to complete the battery preparation.
[0220] [Example 2]
[0221] The perovskite crystalline silicon stacked cell of Example 2 is prepared by referring to the preparation method of Example 1, except that step 8 of Example 2 is replaced by: the inorganic framework layer is fully reacted with the organic salt solution composed of FAI, FABr and MASCN by a slit coating method to obtain a perovskite film, and the perovskite light absorbing layer is obtained after annealing with a thickness of 700 nanometers.
[0222] [Example 3]
[0223] The perovskite crystalline silicon stacked cell of Example 3 is prepared by referring to the preparation method of Example 1, except that step 8 of Example 3 is replaced by: the inorganic framework layer is fully reacted with the organic salt solution composed of FAI and FABr by spin coating to obtain a perovskite film, and the perovskite light absorbing layer is obtained after annealing with a thickness of 700 nanometers.
[0224] [Example 4]
[0225] The perovskite crystalline silicon stacked cell of Example 4 was prepared by referring to the preparation method of Example 1, except that step 8 of Example 4 was replaced by: the inorganic framework layer was allowed to fully react with the organic salt solution composed of FAI and FABr by a slit coating method to obtain a perovskite film, and the perovskite light absorbing layer was obtained after annealing with a thickness of 700 nanometers.
[0226] [Example 5]
[0227] The perovskite crystalline silicon stacked cell of Example 5 is prepared by referring to the preparation method of Example 1, except that step 8 of Example 5 is replaced by: fully reacting the inorganic framework layer with an organic salt solution composed of FAI, FABr and MASCN by spin coating to obtain a perovskite film, and annealing to obtain a perovskite light absorbing layer, wherein the mass ratio of rubidium in the perovskite light absorbing layer is 0.1%, and the thickness of the perovskite light absorbing layer is 700 nanometers.
[0228] [Example 6]
[0229] The perovskite crystalline silicon stacked cell of Example 6 was prepared by referring to the preparation method of Example 1, except that step 8 of Example 6 was replaced by: fully reacting the inorganic framework layer with an organic salt solution composed of FAI, FABr and MASCN by spin coating to obtain a perovskite film, and annealing to obtain a perovskite light absorbing layer, wherein the mass ratio of rubidium in the perovskite light absorbing layer was 1%, and the thickness of the perovskite light absorbing layer was 700 nanometers.
[0230] [Example 7]
[0231] The perovskite crystalline silicon stacked cell of Example 7 was prepared by referring to the preparation method of Example 1, except that step 8 of Example 7 was replaced by: the inorganic framework layer was allowed to fully react with an organic salt solution composed of FAI, FABr and MASCN by spin coating to obtain a perovskite film, and the perovskite light absorbing layer was obtained after annealing, wherein the mass ratio of rubidium in the perovskite light absorbing layer was 0.05%, and the thickness of the perovskite light absorbing layer was 700 nanometers.
[0232] [Example 8]
[0233] The perovskite crystalline silicon stacked cell of Example 8 is prepared by referring to the preparation method of Example 1, except that step 8 of Example 8 is replaced by: fully reacting the inorganic framework layer with an organic salt solution composed of FAI, FABr and MASCN by spin coating to obtain a perovskite film, and annealing to obtain a perovskite light absorbing layer, wherein the mass ratio of rubidium in the perovskite light absorbing layer is 1.5%, and the thickness of the perovskite light absorbing layer is 700 nanometers.
[0234] [Example 9]
[0235] The perovskite crystalline silicon stacked cell of Example 9 is prepared by referring to the preparation method of Example 1, except that step 7 of Example 9 is replaced by: using a three-source co-evaporation method to evaporate PbI2, CsBr, and RbI on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0236] [Example 10]
[0237] The perovskite crystalline silicon stacked cell of Example 10 is prepared by referring to the preparation method of Example 1, except that step 7 of Example 10 is replaced by: using a three-source co-evaporation method to evaporate PbI2, CsBr, and RbBr on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0238] [Example 11]
[0239] The perovskite crystalline silicon stacked cell of Example 11 is prepared by referring to the preparation method of Example 1, except that step 7 of Example 11 is replaced by: using a three-source co-evaporation method to evaporate PbI2, CsCl, and RbCl on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0240] [Example 12]
[0241] The perovskite crystalline silicon stacked cell of Example 12 is prepared by referring to the preparation method of Example 1, except that step 7 of Example 12 is replaced by: using a three-source co-evaporation method to evaporate PbI2, CsI, and RbCl on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0242] [Comparative Example 1]
[0243] The perovskite crystalline silicon stacked cell of Comparative Example 1 is prepared by referring to the preparation method of Example 1, except that step 7 of Comparative Example 1 is replaced by: using double co-evaporation method to evaporate PbI2 and CsBr on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0244] [Comparative Example 2]
[0245] The perovskite crystalline silicon stacked cell of Comparative Example 2 is prepared by referring to the preparation method of Example 1, except that step 7 of Comparative Example 2 is replaced by: using double co-evaporation method to evaporate PbI2 and CsCl on the hole transport layer to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0246] [Comparative Example 3]
[0247] The perovskite crystalline silicon stacked cell of Comparative Example 3 was prepared by referring to the preparation method of Example 1, except that step 7 of Comparative Example 3 was replaced by: PbI2 and CsI were evaporated on the hole transport layer by double co-evaporation to form a mixed inorganic framework layer with a thickness of 400 nanometers.
[0248] The test data is shown in Table 1:
[0249]
[0250]
[0251] Table 1
[0252] It can be seen from Table 1 above that the perovskite crystalline silicon tandem cells prepared by the methods in Examples 1 to 12 have better performance and stability than the perovskite crystalline silicon tandem cells prepared by the methods in Comparative Examples 1 to 3.
[0253] The embodiment of the present application may also provide a photovoltaic module (not shown), including at least one battery string, the battery string includes at least two perovskite crystalline silicon stacked batteries as described above, and adjacent perovskite crystalline silicon stacked batteries can be connected together by series welding.
[0254] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0255] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0256] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0257] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0258] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing a perovskite light-absorbing layer, characterized in that: include: Providing a suede substrate, on which a first compound, a second compound and a third compound are co-evaporated from three sources to form an inorganic framework layer, wherein the first compound is lead iodide, the second compound is cesium iodide, cesium bromide or cesium chloride, and the third compound is rubidium chloride, rubidium iodide or rubidium bromide; coating an organic salt solution on the inorganic framework layer by a spin coating method or a slit coating method to obtain a perovskite film; The perovskite film is annealed to obtain a perovskite light absorbing layer.
2. The method for preparing a perovskite light absorbing layer according to claim 1, characterized in that: In the perovskite light-absorbing layer, the mass ratio of rubidium is 0.1%-1%; And / or, the thickness of the perovskite light absorbing layer is 400-800 nanometers.
3. The method for preparing a perovskite light absorbing layer according to any one of claims 1 to 2, characterized in that: The preparation of the suede substrate comprises: Provide crystalline silicon bottom cells; A tunneling layer and a hole transport layer are sequentially prepared on the crystalline silicon bottom cell to obtain the velvet substrate.
4. The method for preparing a perovskite light absorbing layer according to claim 3, characterized in that: The preparation of the crystalline silicon bottom cell includes: Providing an N-type silicon wafer substrate with a velvet surface, wherein the silicon wafer substrate has a first surface and a second surface opposite to each other; Sequentially preparing a first intrinsic amorphous silicon layer and an N-type amorphous silicon layer on the first surface of the silicon wafer substrate; A second intrinsic amorphous silicon layer, a P-type amorphous silicon layer, a first conductive layer and a first metal electrode layer are sequentially prepared on the second surface of the silicon wafer substrate.
5. The method for preparing a perovskite light absorbing layer according to claim 4, characterized in that: The first conductive layer is a first transparent conductive oxide layer; And / or, the tunneling layer is a second transparent conductive oxide layer.
6. The method for preparing a perovskite light absorbing layer according to claim 1, characterized in that: The thickness of the inorganic framework layer is 300-500 nanometers.
7. The method for preparing a perovskite light absorbing layer according to claim 1, characterized in that: The preparation of the organic salt solution comprises: Dissolve formamidine iodine, formamidine bromide and methylamine thiocyanate in isopropyl acetone solvent; The isopropyl ketone solvent is stirred until the formamidine iodine, the formamidine bromide, and the methylammonium thiocyanate are completely dissolved to obtain the organic salt solution, wherein the concentration of the formamidine iodine is within a first preset range, the concentration of the formamidine bromide is within a second preset range, and the concentration of the methylammonium thiocyanate is within a third preset range.
8. A method for preparing a perovskite crystalline silicon tandem battery, characterized in that: include: Preparing a perovskite light absorbing layer, wherein the perovskite light absorbing layer is prepared by the method for preparing a perovskite light absorbing layer according to any one of claims 1 to 7; An electron transport layer, a second conductive layer and a second metal electrode layer are sequentially prepared on the perovskite light-absorbing layer to obtain a perovskite crystalline silicon stacked cell.
9. The method for preparing a perovskite crystalline silicon tandem cell according to claim 8, characterized in that: The method further comprises: A buffer layer is prepared between the electron transport layer and the second conductive layer.
10. The method for preparing a perovskite crystalline silicon tandem cell according to claim 9, characterized in that: The method further comprises: A buffer modification layer is prepared between the buffer layer and the electron transport layer.
11. The method for preparing a perovskite crystalline silicon tandem battery according to claim 11, wherein the material of the buffer modification layer is at least one of zinc oxide aluminum, zinc oxide, and tungsten oxide nanoparticles; And / or, the thickness of the buffer modification layer is 1-10 nanometers.
12. A perovskite crystalline silicon tandem battery, characterized in that: include: A suede substrate, and a perovskite light absorbing layer, an electron transport layer, a second conductive layer and a second metal electrode layer stacked in sequence on the suede substrate, wherein the perovskite light absorbing layer is prepared by the perovskite light absorbing layer preparation method according to any one of claims 1 to 7.
13. A photovoltaic module, characterized in that: include: At least one battery string, the battery string comprising at least two perovskite crystalline silicon stacked cells as claimed in claim 12.
14. A photovoltaic system, characterized in that: The photovoltaic system comprises the photovoltaic assembly according to claim 13.
Citation Information
Cited By
Perovskite solar cell and preparation method thereof
CN120035355A