Method for manufacturing transfer foil based on composite printing and transfer foil
By combining screen printing and digital printing technology in the transfer foil, a multi-layer structure transfer foil is formed, which solves the design and cost problems in extremely small batch manufacturing, and achieves efficient and environmentally friendly transfer foil production.
Patent Information
- Application Number
- CN202380014810.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-15
AI Technical Summary
The existing transfer foils are difficult to improve designability when manufactured in very small batches, and there are problems such as printing alignment accuracy, extended delivery time, and increased costs, especially in the composite use of gravure and screen printing.
Using the transfer foil manufacturing method of the peeling layer, color ink layer, shielding layer and adhesive layer sequentially on the support sheet, the shielding layer and the adhesive layer are formed by screen printing, and the color ink layer is formed by digital printing, combined with screen printing. High shading performance and the thickness of digital printing realize multi-color one-time design.
It has achieved the improvement of the design of transfer foil in extremely small batch production, shortened the lead time, reduced the plate making cost, reduced the amount of solvent used, and improved production efficiency and environmental friendliness.
Smart Images

Figure CN118973809A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a transfer foil and a transfer foil, and more particularly, to a method for producing a transfer foil using screen printing and digital printing in combination and a transfer foil. Background Art
[0002] Conventionally, as a method for decorating the surface of a transfer object with a pattern, color, etc., a method using a transfer foil is used, wherein the transfer foil is formed by laminating a transfer layer such as a peeling layer, a color ink layer, and an adhesive layer on a support sheet. Such a transfer foil is required to improve the design properties in order to improve the product image of the transfer object after the decoration obtained by transfer.
[0003] Regarding the printing method of each layer, sometimes a single printing method is used, and sometimes a combination of multiple printing methods is used. When printing in combination, it is necessary to align the printing position. If it is a printing method between the same rotary methods, alignment is easy, but Roll-to-Roll screen printing is intermittent feeding, so it is difficult to combine with the rotary method.
[0004] In addition, Patent Document 1 discloses a transfer foil having a peeling layer, a polarizing ink layer, a color ink layer, and a thermosensitive adhesive layer laminated in sequence on the side of a base film, characterized in that as the polarizing ink forming the polarizing ink layer, an ink in which 10 to 15% by weight of pearl pigment is added to a transparent resin is used, and both sides of the polarizing ink layer are covered with a two-liquid curing primer. According to this transfer foil, by having a specific polarizing ink layer, a pearl luster is given to the pattern, and a decorative effect higher than that of the color ink pattern can be exerted.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 7-40651 Summary of the invention
[0008] The formation of each layer responsible for the design of the transfer foil is usually carried out by gravure printing (large batches), screen printing (small to medium batches), etc. However, in reality, there are many cases where very small batches are required to be manufactured. In terms of design, it is often necessary to improve the design by combining the grayscale expression that is a characteristic of gravure printing, the high shielding expression that is a characteristic of screen printing, and the functional ink expression. However, for the composite transfer foil of gravure printing and screen printing, not only is it impossible to cope with very small batches, but there are also problems such as the problem of printing alignment accuracy, longer delivery time, and rising costs (rising plate costs, rising film costs, and rising ink costs), which is not realistic.
[0009] An object of the present disclosure is to provide a method for producing a transfer foil and a transfer foil capable of producing a transfer foil having improved designability in a plurality of designs and a plurality of color tones at once in an extremely small batch without being restricted by a plate.
[0010] A method for manufacturing a transfer foil in one embodiment of the present disclosure is a method for manufacturing a transfer foil in which a peeling layer, a color ink layer, a shielding layer, and an adhesive layer are sequentially stacked on one side of a support sheet. The shielding layer and the adhesive layer are respectively formed by screen printing, and the color ink layer is formed by digital printing.
[0011] A transfer foil according to one embodiment of the present disclosure includes a support sheet, a peeling layer, a color ink layer, a shielding layer, and an adhesive layer laminated in this order. The shielding layer and the adhesive layer are each composed of a screen printing layer, and the color ink layer is composed of a digital printing layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a flowchart showing the method for producing the transfer foil according to the present embodiment.
[0013] Figure 2 This is a schematic cross-sectional view showing an example of the transfer foil according to the present embodiment.
[0014] Figure 3 This is a schematic cross-sectional view showing another example of the transfer foil according to the present embodiment.
[0015] Figure 4 This is a schematic cross-sectional view showing another example of the transfer foil according to the present embodiment. DETAILED DESCRIPTION
[0016] The following describes the embodiments of the present disclosure. In addition, the present disclosure is not limited to the following embodiments. The following embodiments are only a part of various embodiments of the present disclosure, and various changes can be made according to the design as long as the purpose of the present disclosure can be achieved.
[0017] The method for producing a transfer foil according to the present embodiment is for producing a transfer foil in which a release layer, a color ink layer, a shielding layer, and an adhesive layer are sequentially laminated on one side of a support sheet.
[0018] The present inventors have conducted intensive research on methods for improving the design of transfer foils and have found that by using a specific combination of printing methods for each layer constituting the transfer foil, the design can be improved and is also suitable for very small batch production, thereby completing the present disclosure.
[0019] <Method for Manufacturing Transfer Foil>
[0020] In the method for manufacturing the transfer foil of the present embodiment (hereinafter also referred to as manufacturing method (X)), in the method for manufacturing a transfer foil in which a peeling layer, a color ink layer, a shielding layer and an adhesive layer are sequentially stacked on one side of a support sheet, the shielding layer and the adhesive layer are respectively formed by screen printing, and the color ink layer is formed by digital printing.
[0021] In the manufacturing method (X), in addition to the above-mentioned layers, other shielding layers and / or anchoring layers may be further formed. The flow chart of the manufacturing method (X) including the formation of other shielding layers and anchoring layers is shown in Figure 1 .
[0022] Figure 1 The manufacturing method (X) shown in the process includes, in sequence, a peeling layer forming step (S1), another shielding layer forming step (S11), a color ink layer forming step (S2), an anchoring layer forming step (S12), a shielding layer forming step (S3) and an adhesive layer forming step (S4).
[0023] In the manufacturing method (X), the shielding layer 40 and the adhesive layer 50 are respectively formed by screen printing, and the color ink layer 30 is formed by digital printing.
[0024] Figure 2 to Figure 4 This is a cross-sectional view showing an example of the transfer foil produced by the production method (X).
[0025] Figure 2 The transfer foil 1 includes a support sheet 10 , a release layer 20 , another shielding layer 110 , a color ink layer 30 , an anchor layer 120 , a shielding layer 40 , and an adhesive layer 50 . Figure 3 The transfer foil 1 includes a support sheet 10 , a release layer 20 , a color ink layer 30 , an anchor layer 120 , a shielding layer 40 , and an adhesive layer 50 . Figure 4 The transfer foil 1 includes a support sheet 10 , a release layer 20 , a color ink layer 30 , a shielding layer 40 , and an adhesive layer 50 .
[0026] Figure 2 The transfer foil 1 includes another shielding layer 110 between the release layer 20 and the color ink layer 30. In addition, an anchoring layer 120 is provided between the color ink layer 30 and the shielding layer 40. In the manufacturing method (X), when the transfer foil 1 includes another shielding layer 110, it is preferred to form the other shielding layer 110 by screen printing. In addition, when the transfer foil 1 includes an anchoring layer 120, it is preferred to form the anchoring layer 120 by screen printing.
[0027] In this way, by setting the printing method of each layer constituting the transfer foil to a specific printing method, the design of the obtained transfer foil can be improved. The reason why the manufacturing method (X) has such a structure to achieve the effect of improving the design is that, for example, the advantages of screen printing (high shielding performance, high chroma, gold, silver, pearl color, etc.) and the advantages of digital printing (shade performance, fine line performance, grayscale performance, photo image reproducibility, etc.) are effectively combined. In addition, since digital printing does not require a plate, the data can be freely adjusted in shade, fine line, and grayscale at the printing site, and multiple changed patterns can be combined and printed at one time, so as to confirm or propose.
[0028] In addition, since the manufacturing method (X) is a method combining screen printing and digital printing, it is different from the conventional transfer foil manufacturing method which is suitable for mass production and forms each layer by gravure printing, etc., and can well cope with the production of very small batches. Since it is suitable for such a very small batch manufacturing method, it is possible to shorten the delivery time, produce a variety of products, and make it easier and faster to plan based on a variety of samples, etc. The color ink layer of digital printing does not require a plate, which can shorten the conventional plate making time.
[0029] Furthermore, according to the manufacturing method (X), compared with the conventional transfer foil manufacturing method using gravure printing or the like, it is possible to achieve a significant reduction in plate making costs, and the amount of solvent used in the manufacturing can also be significantly reduced, and the effect of reducing environmental load can also be achieved. In addition, in conventional gravure printing and screen printing, when a customer performs color correction of a new product pattern, it is necessary to perform color management, plate replacement, and color tone adjustment multiple times within a few days, but with digital printing, samples after multiple color adjustments and design adjustments can be seen at once on the spot, so that a decision can be made immediately, and the lead time for the launch of new products can be shortened.
[0030] Hereinafter, each step will be described.
[0031] [Peeling layer forming step (S1)]
[0032] In this step (S1), a release layer 20 is formed on one side of the support sheet 10. The release layer 20 is provided to improve the releasability between the support sheet 10 and the color ink layer 30 or other shielding layer 110 and to improve the transferability of the transfer foil 1 to the transfer object.
[0033] The support sheet 10 preferably has flexibility, heat resistance so as not to be easily softened and deformed by heat pressing in a thermal transfer process or the like, mechanical strength, chemical resistance, and the like.
[0034] As the material of the support sheet 10, for example, polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, synthetic resins such as polyvinyl chloride, polycarbonate, poly(meth)acrylate, polystyrene, polyethylene, polypropylene, triacetyl cellulose, polyvinyl alcohol, and polyimide, natural resins, paper, synthetic paper, and composites thereof can be cited. Among them, polyester is preferred, and polyethylene terephthalate is more preferred. The support sheet 10 is preferably roughened by silicone resin or the like.
[0035] As the support sheet 10, a long sheet is generally used. From the viewpoint of maintaining sufficient flexibility, the thickness of the support sheet 10 is preferably 19 μm or more and 100 μm or less, and more preferably 25 μm or more and 70 μm or less. In addition, for example, as required, it is preferred to apply a release agent such as silicone, melamine, alkyd, or UV-curable polyol resin on the surface of the support sheet 10 for use.
[0036] In step (S1), the method for forming the peeling layer 20 is not particularly limited, and it can be formed by, for example, screen printing, gravure printing, etc., but it is preferred to form the peeling layer 20 by screen printing. "Screen printing" is a type of stencil printing, and is a printing method that uses a screen printing plate with a fine mesh woven from synthetic fibers such as polyester, metal fibers such as stainless steel, etc., and passes ink through the mesh to print on an object. In screen printing, a screen printing plate with a mesh corresponding to the pattern, thickness, etc. of each layer to be formed is used.
[0037] In the step (S1), when the release layer 20 is formed by screen printing, the ink used (hereinafter also referred to as ink (S1)) preferably has low adhesion to the support sheet 10, and moderate adhesion to the color ink layer 30 or other shielding layer 110. As the components of the ink (S1), for example, vinyl chloride-vinyl acetate resin (vinyl chloride-vinyl acetate resin), urethane resin, acrylic resin, polyester resin, etc. can be cited. The ink (S1) may contain a curing agent. As the ink (S1), polyester is preferred from the viewpoint of making the adhesion to the color ink layer 30 or other shielding layer 110 more moderate. When the ink (S1) contains a solvent, the solvent used is preferably cyclohexanone, isophorone, a high boiling point aromatic solvent, etc. in the case of screen printing, and preferably toluene, methyl ethyl ketone, ethyl acetate, etc. in the case of gravure printing. In addition, when printing the ink (S1) on the support sheet 10, it is preferred to use an additive for improving the leveling property of the ink coating and the defoaming property of the ink.
[0038] Usually, the release layer 20 formed in step ( S1 ) is a layer having a substantially uniform thickness. The thickness of the release layer 20 is, for example, 0.5 μm to 5 μm, and preferably 0.7 μm to 3 μm.
[0039] [Other shielding layer forming step (S11)]
[0040] In this step (S11), another hidden layer 110 is formed on the surface of the peeling layer 20. The other hidden layer 110 is provided to conceal the color and pattern of the transferred object to improve the design, or when decoration of gold, silver, pearl, etc. is required. Examples of the color of the other hidden layer 110 include white, black, yellow, red, blue, gold, silver, pearl, etc.
[0041] In this step ( S11 ), the method for forming the other hiding layer 110 is not particularly limited, and the other hiding layer 110 may be formed by, for example, screen printing, gravure printing, etc. However, it is preferred that the other hiding layer 110 is formed by screen printing.
[0042] In the step (S11), when the other shielding layer 110 is formed by screen printing, the ink used (hereinafter, also referred to as ink (S11)) preferably has appropriate adhesion to the color ink layer 30. Examples of the ink (S11) include a material obtained by mixing a colorant such as a pigment or dye, a body pigment, a stabilizer, a plasticizer, a catalyst, a curing agent, an antioxidant, an ultraviolet absorber, and the like in a resin binder.
[0043] Examples of the resin binder include butyral resin, polyamide resin, polyethyleneimine resin, sulfonamide resin, polyester polyol resin, petroleum resin, epoxy resin, styrene resin, acrylic resin, vinyl chloride resin, etc. Examples of the colorant include: inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, chrome yellow, titanium yellow, red iron oxide, cadmium red, ultramarine, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, and phthalocyanine blue; metallic pigments composed of flaky foils such as aluminum and brass; and pearlescent (pearl) pigments composed of flaky foils such as titanium dioxide-coated mica and basic lead carbonate.
[0044] As a component of the ink (S11), vinyl chloride-vinyl acetate / polyester resin is preferred from the viewpoint of achieving more appropriate adhesion with the color ink layer 30. When the ink (S11) contains a solvent, the solvent used is preferably cyclohexanone, isophorone, a high-boiling point aromatic solvent, etc. in the case of screen printing.
[0045] The other hidden layer 110 formed in step ( S11 ) is generally a layer having a substantially uniform thickness. The thickness of the other hidden layer 110 is preferably 0.5 μm to 5 μm, and more preferably 0.7 μm to 3 μm per color.
[0046] [Color ink layer forming step (S2)]
[0047] In this step (S2), a color ink layer 30 is formed by digital printing on the surface of the release layer 20 or other masking layer 110. The color ink layer 30 is a layer for providing the transfer foil 1 with decoration such as a pattern or color.
[0048] "Digital printing" refers to a method of printing directly from a digitized image onto various substrates. Examples of digital printing include inkjet printing and laser printing. "Inkjet printing" is, for example, a printing method that uses a print head that uses a piezoelectric crystal to eject droplets of ink, thereby causing the droplets to accumulate on a substrate to reproduce a digital image. "Laser printing" is a printing method that uses a toner to expose the required pixels with a laser, temporarily holds the toner, and then heat-fixes it onto a substrate to reproduce a digital image.
[0049] In the digital printing of step (S2), inks or toners of various colors such as yellow (Y), magenta (M), cyan (C), black (K), and white (W) are usually used. The ink can be prepared by mixing pigments such as coloring pigments and fluorescent pigments with resin binders. In addition, the ink can contain a release agent, a softener, a surfactant, etc. As coloring pigments, various well-known pigments can be used, for example, carbon black, azo, phthalocyanine, quinacridone, thioindigo, anthraquinone, isoindolinone and other pigments can be cited. As a resin binder, for example, the same resin binder as the resin binder exemplified as the binder of the ink forming the other shielding layer 110 can be cited.
[0050] In the digital printing in step (S2), a toner is preferably used, and a polyester-based toner is more preferably used.
[0051] As digital printing, laser printing using toner is preferred from the viewpoint of printing speed. In the case of laser printing using toner, the thickness of the color ink layer 30 is preferably 3 μm to 12 μm per color, more preferably 4 μm to 10 μm.
[0052] [Anchor layer forming step (S12)]
[0053] In this step ( S12 ), the anchor layer 120 is formed on the surface of the color ink layer 30 . The anchor layer 120 is provided to protect the color ink layer 30 and to make the color ink layer 30 and the shielding layer 40 adhere to each other.
[0054] In this step ( S12 ), the method for forming the anchor layer 120 is not particularly limited, and the anchor layer 120 may be formed by, for example, screen printing, gravure printing, etc. However, it is preferred that the anchor layer 120 be formed by screen printing.
[0055] In the step (S12), when the anchor layer 120 is formed by screen printing, the ink used (hereinafter also referred to as ink (S12)) preferably has moderate adhesion to the color ink layer 30. As the components of the ink (S12), for example, thermoplastic resins such as vinyl chloride-vinyl acetate resins (vinyl chloride-vinyl acetate resins), urethane resins, polyester resins, and vinyl chloride-vinyl acetate / polyester resins can be cited. As the components of the ink (S12), from the viewpoint of making the adhesion to the color ink layer 30 more moderate, vinyl chloride-vinyl acetate / polyester resins are preferred. The ink (S12) may contain a curing agent. The ink (S12) usually contains a solvent. As the solvent, for example, aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, alcohol solvents, glycol solvents, etc. can be cited. As the solvent contained in the ink (S12), from the viewpoint of suppressing the redissolution of the color ink layer 30, aromatic hydrocarbon solvents are preferred.
[0056] The anchor layer 120 formed in the step ( S12 ) is generally a layer having a substantially uniform thickness. The thickness of the anchor layer 120 is, for example, 0.5 μm to 4.0 μm, and preferably 1.0 μm to 3.5 μm.
[0057] [Shielding layer forming step (S3)]
[0058] In this step (S3), a shielding layer 40 is formed by screen printing on the surface of the anchor layer 120. The shielding layer 40 is provided to shield the color and pattern of the transferred object to improve the design, or when decoration of gold, silver, pearl, etc. is required. Examples of the color of the shielding layer 40 include white, black, yellow, red, blue, gold, silver, pearl, etc.
[0059] The ink (hereinafter also referred to as ink (S3)) used in the screen printing of step (S3) preferably has moderate adhesion to the anchor layer 120 when the transfer foil 1 has the anchor layer 120, and preferably has moderate adhesion to the color ink layer 30 when the transfer foil 1 does not have the anchor layer 120. As the components of the ink (S3), for example, a material obtained by mixing a colorant such as a pigment or a dye, a body pigment, a stabilizer, a plasticizer, a catalyst, a curing agent, an antioxidant, an ultraviolet absorber, etc., with a thermoplastic resin binder such as a vinyl chloride-vinyl acetate resin (vinyl chloride-vinyl acetate resin), a urethane resin, a polyester resin, and a vinyl chloride-vinyl acetate / polyester resin can be cited. The ink (S3) may contain a curing agent. In addition, the ink (S3) usually contains a solvent. As the solvent contained in the ink (S12), an aromatic hydrocarbon solvent is preferred from the viewpoint of suppressing the redissolution of the color ink layer 30.
[0060] As the resin binder, for example, the same resin binder as the resin binder exemplified as the binder of the ink (S11) forming the other shielding layer 110 can be cited. As the colorant, for example, the same colorant as the colorant exemplified as the colorant of the ink (S11) forming the other shielding layer 110 can be cited.
[0061] When the transfer foil 1 does not include the anchor layer 120, as a component of the ink (S3), from the viewpoint of achieving more appropriate adhesion with the color ink layer 30, preferably a vinyl chloride-vinyl acetate resin, a polyester resin, and a vinyl chloride-vinyl acetate / polyester resin, and more preferably a vinyl chloride-vinyl acetate / polyester resin. From the viewpoint of suppressing the redissolution of the color ink layer 30, the solvent contained in the ink (S3) is preferably an aromatic hydrocarbon solvent.
[0062] The shielding layer 40 formed in step ( S3 ) is generally a layer having a uniform thickness. The thickness of the shielding layer 40 is preferably 0.5 μm to 5 μm, and more preferably 0.7 μm to 3 μm per color.
[0063] [Adhesive layer forming step (S4)]
[0064] In this step (S4), the adhesive layer 50 is formed by screen printing on the surface of the shielding layer 40. The adhesive layer 50 is provided for adhesion when transferring from the transfer foil 1 to the transfer target.
[0065] The ink used for screen printing in step (S4) (hereinafter also referred to as ink (S4)) preferably has moderate adhesion to the shielding layer 40, and further preferably has moderate adhesion to the components to be bonded in the thermal transfer step after printing. The components to be bonded in the thermal transfer step are not particularly limited, and examples thereof include organic substances such as plastics and natural materials, and inorganic substances such as glass, metals, and ceramics. For components containing such components, thermoplastic resins and hot melt adhesives are preferred as components of the ink (S4). When the ink (S4) contains a solvent, an aromatic hydrocarbon solvent is preferred as the solvent from the viewpoint of suppressing the redissolution of the color ink layer 30.
[0066] As thermoplastic adhesives, for example, two-component curing urethane adhesives, polyester urethane adhesives, polyether urethane adhesives, acrylic adhesives, polyester adhesives, polyamide adhesives, polyvinyl acetate adhesives, epoxy adhesives, rubber adhesives, etc. are listed, but in order to make the adhesion with the shielding layer 40 moderate, it is preferred to use, for example, vinyl chloride-vinyl acetate resins (vinyl chloride-vinyl acetate resins), urethane resins, polyester resins, vinyl chloride-vinyl acetate / polyester resins, acrylic resins, etc.
[0067] As the hot melt adhesive, for example, resins such as ethylene-vinyl acetate, vinyl chloride-vinyl acetate (vinyl chloride-vinyl acetate), polyolefin, polyamide, nylon, polyester, rubber, acrylic, urethane, cellulose, and reactive hot melt can be cited, and a mixture of two or more can be used as required. It is particularly preferred to use a mixture of acrylic resin and polyurethane resin.
[0068] The ink (S4) may contain additives such as a pigment, a dye, an antioxidant, a curing agent, a catalyst, a leveling agent, a defoaming agent, a thixotropic agent, an extender pigment, and an ultraviolet absorber.
[0069] From the viewpoint of improving the adhesion to the transferred object, the ink (S4) is preferably made of the same system as the material constituting the transferred object. As the components of the ink (S4), polyester resins and vinyl chloride-vinyl acetate / polyester resins are preferred.
[0070] Generally, the adhesive layer 50 formed in step ( S4 ) is a layer having a substantially uniform thickness. The thickness of the adhesive layer 50 is, for example, 0.6 μm to 8 μm, preferably 2 μm to 5 μm.
[0071] <Transfer Foil Manufacturing Apparatus>
[0072] As a manufacturing device for performing the manufacturing method (X) (hereinafter, also referred to as manufacturing device (Y)), for example, a combination of a screen printer for performing screen printing and a digital printer for performing digital printing can be cited. The manufacturing device (Y) can be, for example, a device having a screen printing unit and a digital printing unit, or an existing digital printer and an existing digital printer can be used to perform the manufacturing method (X). In this case, by using an existing device, the device cost can be reduced.
[0073] Screen printing machines are usually intermittent feed machines. Digital printing machines include, for example, rotary printing machines and continuous feed machines. As a manufacturing device (Y), the screen printing machine is of intermittent feed type, and the digital printing machine is preferably of rotary type. This is because in the combination of rotary type and continuous feed type, it is difficult to repeatedly perform multiple offline printings to ensure output position accuracy, but in an intermittent feed screen printing machine, position correction can be performed multiple times offline for printing. In addition, compared with rotary methods such as gravure printing, the screen printing machine uses less ink at the beginning of printing and has a low plate making cost. Therefore, in terms of printing small quantities and multiple varieties, it has good compatibility with digital printing. In this way, the manufacturing device (Y) can further realize the collaboration between the screen printing machine and the digital printing machine, and can more easily manufacture the transfer foil 1.
[0074] When the digital printer for forming the color ink layer 30 is a rotary type, during the digital printing process, the support sheet 10 of the transfer foil being manufactured may expand and contract in both the conveying direction and the width direction, resulting in deformation of the shape of the pattern in the color ink layer 30. In order to cope with such a situation, in screen printing after forming the anchor layer 120 or the shielding layer 40, it is preferable to be able to calibrate the size, material, and elasticity of the screen printing plate in a manner that matches the deformation.
[0075] <Transfer Foil>
[0076] like Figure 2 to Figure 4 As shown, the transfer foil (hereinafter also referred to as transfer foil (Z)) 1 of this embodiment is sequentially stacked with a support sheet 10, a peeling layer 20, a color ink layer 30, a shielding layer 40 and an adhesive layer 50. The shielding layer 40 and the adhesive layer 50 are respectively composed of screen printing layers, and the color ink layer 30 is composed of a digital printing layer.
[0077] The transfer foil (Z) 1 may further include another shielding layer 110 between the release layer 20 and the color ink layer 30, and may further include an anchoring layer 120 between the color ink layer 30 and the shielding layer 40. In this case, the other shielding layer 110 is preferably formed of a screen printing layer, and the anchoring layer 120 is preferably formed of a screen printing layer.
[0078] The transfer foil (Z) 1 is a layer in which the shielding layer 40 and the adhesive layer 50 are formed by screen printing, and the color ink layer 30 is a layer formed by digital printing, so that the design property can be improved.
[0079] Example
[0080] Hereinafter, the present disclosure will be specifically described by way of examples, but the present disclosure is not limited only to the examples.
[0081] <Manufacturing of transfer foil>
[0082] [Manufacturing of transfer foil 1]
[0083] We manufacture transfer foil (for coated containers) using screen printers and digital printers.
[0084] Support sheet: Polyethylene terephthalate film (thickness 25 μm, film surface subjected to release treatment) The coating materials used in forming each layer are as follows.
[0085] ·Peel layer: polyester resin (thickness: 3μm)
[0086] Color ink layer: Toner (polyester) (cyan, magenta, yellow, black, white)
[0087] Anchor layer: polyester resin (thickness: 3 μm)
[0088] ·Shielding layer: polyester resin (thickness: 3μm)
[0089] Adhesive layer: polyester resin (thickness: 3μm)
[0090] [Manufacturing of transfer foil 2]
[0091] We manufacture transfer foil (thin axis specifications) using screen printing machines and digital printing machines.
[0092] Support sheet: Polyethylene terephthalate film (thickness 25 μm, film surface subjected to release treatment) The coating materials used in forming each layer are as follows.
[0093] ·Peel layer: Vinyl chloride-vinyl acetate resin (thickness: 3 μm)
[0094] Color ink layer: Toner (polyester) (cyan, magenta, yellow, black, white)
[0095] Anchor layer: Vinyl chloride-vinyl acetate resin (thickness: 3 μm)
[0096] ·Shielding layer: Vinyl chloride-vinyl acetate resin (thickness: 3μm)
[0097] Adhesive layer: Vinyl chloride-vinyl acetate / polyester resin (thickness: 3μm)
[0098] [Manufacturing of transfer foil 3]
[0099] We manufacture transfer foil (for molded plastic containers) using screen printers and digital printers.
[0100] Support sheet: Polyethylene terephthalate film (thickness 25 μm, film surface subjected to release treatment) The coating materials used in forming each layer are as follows.
[0101] ·Peel layer: Acrylic resin (thickness: 3μm)
[0102] Color ink layer: Toner (polyester) (cyan, magenta, yellow, black, white)
[0103] Anchor layer: Vinyl chloride-vinyl acetate / polyester resin (thickness: 3μm)
[0104] ·Shielding layer: Vinyl chloride-vinyl acetate / polyester resin (thickness: 3μm)
[0105] Adhesive layer: Vinyl chloride-vinyl acetate / polyester resin (thickness: 3μm)
[0106] <Evaluation>
[0107] [Manufacturing method]
[0108] The transfer foil production method of the present invention was evaluated for the functionality (adhesion) of the obtained transfer foil, the productivity (printability) of the production method, and the processability (transferability) of the transfer foil by the following methods and criteria. The evaluation results are shown in Table 1 below.
[0109] Adhesion: The color ink layer on the surface of the product obtained using the transfer foil was subjected to an adhesion test (cross-cut method) (JIS K5600-5-6 (ISO2409)), and the adhesion was evaluated as follows: A (good): no peeling of the color ink layer was observed, and B (bad): peeling of the color ink layer was observed.
[0110] Printing suitability: In mass production printing, it is judged whether the pattern can stably print qualified products without defects such as scratches, gaps, dirt, blurring, bleeding, unevenness, pinholes, peeling, and adhesion. The printing suitability is evaluated as follows. The evaluation is A (good): printing continues without defects, and B (bad): defects occur and qualified products cannot be printed continuously.
[0111] Transferability: The components to be closely attached (manufacturing 1: coated container, manufacturing 2: plastic thin shaft component, manufacturing 3: plastic container) are subjected to thermal transfer processing (temperature: 180-280°C, pressure: 5-40 kgf / cm 2 ), poor appearance such as poor pattern transfer, scratches, defects, flattening, brightness changes, and reduced yields such as reduced transfer processing speed were judged, and the transferability was evaluated as follows. Evaluation was A (good): no defects occurred and transfer continued, B (bad): transfer defects occurred and qualified products could not be transferred continuously.
[0112] [Table 1]
[0113]
[0114] As is apparent from the results in Table 1, according to the production method of the present invention, a transfer foil having excellent functionality and processability can be produced with good productivity.
[0115] [Design]
[0116] The design of the transfer foil obtained by the manufacturing method of the present invention was evaluated according to the following criteria for grayscale expression, photo image reproduction, fine line / small text expression, high shielding expression, and gold / silver / pearl color expression. The same transfer foil obtained by gravure printing or screen printing was also evaluated in the same manner. The evaluation results are shown in Table 2 below.
[0117] Grayscale expression: The grayscale expression obtained by transfer was evaluated as A (good): no color unevenness and smooth grayscale expression, or B (bad): color unevenness occurred and grayscale expression was poor.
[0118] Photographic image reproduction: The following evaluation was performed on the portion of the transferred photographic image: A (good): 175 or more CMYK multiplied dots were expressed, which means good photographic image reproduction was possible; B (poor): Only less than 175 dots were expressed, which means poor photographic image reproduction.
[0119] · Fine line / small text performance: The fine line / small text obtained by transfer was evaluated as follows: A (good): fine lines less than 0.2 mm and small text less than 2 pt were able to achieve good fine line / small text performance, B (bad): only fine lines greater than 0.2 mm and small text greater than 2 pt could be printed, which was poor in fine line / small text performance.
[0120] High shielding performance: The high shielding performance obtained by transfer was evaluated as follows: A (good): good high shielding performance was obtained without being affected by the color of the base during overlapping printing, B (bad): poor high shielding performance was obtained due to the influence of the color of the base during overlapping printing.
[0121] Gold, silver, and pearl color expression: The gold, silver, and pearl color expression obtained by transfer was evaluated as follows: A (good): gold, silver, and pearl color inks can be printed in batches, and good gold, silver, and pearl color expression is achieved; B (bad): gold, silver, and pearl color inks cannot be printed in batches, and the gold, silver, and pearl color expression is poor.
[0122] [Table 2]
[0123]
[0124] As can be seen from the results in Table 2, the transfer foil obtained by the production method of the present invention has improved design properties compared to conventional transfer foils using gravure printing, screen printing, and the like.
[0125] A comparison between the method for producing the transfer foil of the present invention and the conventional technology is shown below.
[0126] Table 3
[0127]
[0128] As can be seen from Table 3, according to this embodiment, a solution can be proposed with a minimum amount of 1 piece, the manufacturing cost can be reduced to 1 / 3 of that of gravure printing and 1 / 2 of that of screen printing, the shortest delivery time can be reduced to 1 / 30 of that of gravure printing and 1 / 3 of that of screen printing, and as an environmental measure, the amount of solvent used can be reduced to 1 / 30 of that of gravure printing and 1 / 4 of that of screen printing.
[0129] (Summarize)
[0130] As can be seen from the above-mentioned embodiments and examples, the first method for manufacturing a transfer foil (1) is a method for manufacturing a transfer foil (1) in which a peeling layer (20), a color ink layer (30), a shielding layer (40) and an adhesive layer (50) are sequentially stacked on one side of a support sheet (10). The shielding layer (40) and the adhesive layer (50) are respectively formed by screen printing, and the color ink layer (30) is formed by digital printing.
[0131] According to the first embodiment, the advantages of screen printing, such as excellent high shielding performance, high color saturation, and the ability to print in colors such as gold, silver, and pearl, and the advantages of digital printing, such as excellent light and dark performance, fine line performance, grayscale (gradation) performance, and photo image reproducibility, are effectively combined, and as a result, the design of the transfer foil (1) can be improved. In addition, since the manufacturing method is a method of combining screen printing and digital printing, there is no restriction on the plate, and the transfer foil can be manufactured in multiple designs and multiple color tones at one time, which can well cope with the production of very small batches.
[0132] In a second method for producing a transfer foil (1), in the first method, an anchor layer (120) is further stacked between the color ink layer (30) and the shielding layer (40), and the anchor layer (120) is formed by screen printing.
[0133] According to the second embodiment, the transfer foil (1) further includes an anchor layer (120) that protects the color ink layer (30) and can include colors such as gold, silver, and pearl, thereby further improving the design properties.
[0134] In the method for producing a transfer foil (1) according to a third aspect, in the first or second aspect, screen printing is performed by an intermittent feed method, and digital printing is performed by a rotary method.
[0135] According to the third aspect, it is possible to achieve cooperation between screen printing and digital printing, and to achieve simpler production of the transfer foil (1).
[0136] The transfer foil (1) of the fourth mode comprises a support sheet (10), a peeling layer (20), a color ink layer (30), a shielding layer (40) and an adhesive layer (50) which are stacked in sequence, wherein the shielding layer (40) and the adhesive layer (50) are respectively composed of screen printing layers, and the color ink layer (30) is composed of a digital printing layer.
[0137] According to the fourth aspect, the advantages of screen printing and digital printing are effectively combined, and as a result, a transfer foil (1) with improved design properties can be obtained.
[0138] In the transfer foil (1) of the fifth aspect, in the fourth aspect, an anchor layer (120) is further provided between the color ink layer (30) and the shielding layer (40), and the anchor layer (120) is composed of a screen printing layer.
[0139] According to the fifth aspect, by providing the anchor layer (120), the design properties can be further improved.
[0140] Description of Reference Numerals
[0141] 1 transfer foil
[0142] 10 Support sheet
[0143] 20 peeling layers
[0144] 30 color ink layers
[0145] 40 shielding layers
[0146] 50 adhesive layers
[0147] 110 Other shielding layers
[0148] 120 anchoring layer
Claims
1. A method for manufacturing a transfer foil, wherein a peeling layer, a color ink layer, a shielding layer and an adhesive layer are sequentially laminated on one side of a support sheet, in, The shielding layer and the bonding layer are respectively formed by screen printing, and the color ink layer is formed by digital printing.
2. The method for producing a transfer foil according to claim 1, wherein: An anchoring layer is also stacked between the color ink layer and the shielding layer. The anchor layer is formed by screen printing.
3. The method for producing a transfer foil according to claim 1 or 2, wherein: The screen printing is performed in an intermittent feeding manner, and the digital printing is performed in a rotary manner.
4. A transfer foil comprising a support sheet, a peeling layer, a color ink layer, a shielding layer and an adhesive layer laminated in this order, wherein: The shielding layer and the adhesive layer are respectively composed of screen printing layers, The color ink layer is composed of a digital printing layer.
5. The transfer foil according to claim 4, wherein An anchor layer is further provided between the color ink layer and the shielding layer, and the anchor layer is composed of a screen printing layer.
Citation Information
Patent Citations
Decorative sheet and decorative resin molded article
JP2015193244A
Image formation device, image formation method and program
JP2021088127A
A manufacturing method of thick digital image sheet having improved durability
KR1020150044756A