Manufacture of multifunctional nanostructures using supercritical CO2 assisted spray deposition
Through supercritical CO2-assisted spray deposition technology and cellulose nanocrystal assisted methods, the problem of difficulty in controlling nanostructure formation in the prior art is solved, and the manufacturing of nanocomposites with high performance and high reproducibility is achieved, and the mechanical properties are improved.
Patent Information
- Application Number
- CN202380029430.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-24
- Filing Date
- 2023-01-20
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to accurately control the formation of microstructures, resulting in poor manufacturing reproducibility and low performance, especially in spray-based processing techniques in large-scale applications.
The supercritical CO2-assisted spray deposition method combined with hybrid nanomaterial systems such as cellulose nanocrystals (CNCs) and carbon nanotubes/graphene nanosheets were prepared through ultrasonic treatment and vacuum-assisted resin transfer molding technology. Hybrid composite materials with amphiphilic properties achieve precise deposition of nanostructures.
Accurate control of nanostructure pattern shape, size and height is achieved, manufacturing reproducibility and performance is improved, costs are reduced, and mechanical properties such as bending and interlayer shear strength are significantly improved in multi-material systems.
Smart Images

Figure CN118973948A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This patent application claims priority to U.S. Provisional Patent Application No. 63 / 302,491 filed on January 24, 2022, and the entire disclosure of which is incorporated herein by reference.
[0003] Statement Regarding Federally Funded Research
[0004] This invention was made with Government support under National Science Foundation Grants 1930277 and 2134456. The Government has certain rights in this invention. Technical Field
[0005] The present disclosure relates generally to the fabrication of two-dimensional and three-dimensional multifunctional nanostructures, and more particularly, but not by way of limitation, to the fabrication of two-dimensional and three-dimensional multifunctional nanostructures using supercritical CO2-assisted spray deposition and evaporation of colloidal droplets. Background Art
[0006] This section provides background information to facilitate a better understanding of various aspects of the present disclosure. It should be understood that the statements in this section of this document should be read in this light, and not as admissions of prior art.
[0007] The integration of nanomaterials (NMs) within various manufacturing technologies enables the production of components with emerging functionality. The lack of control of NM patterns that form microstructures leads to poor manufacturing reproducibility and low performance. To date, there is no high-throughput spray-based processing technology that can accurately control microstructures for large-scale applications. The method disclosed herein overcomes existing challenges by combining a novel and scalable spray deposition method that can control droplet properties with an innovative building block (hybrid nanomaterial system; HNMS) to deposit a desired pattern. Customized nanostructures are composed of these patterns without the need for expensive processing. Summary of the invention
[0008] This Summary is provided to introduce a selection of concepts that are further described below in the Detailed Description. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.
[0009] In one embodiment, the present disclosure relates to a method of depositing a nanostructure having an engineered pattern. Generally, the method includes selecting nanoparticles and a substrate and delivering the nanoparticles to the substrate via a supercritical CO2-assisted atomization (SAA) system.
[0010] In other embodiments, the present disclosure relates to a method for preparing a colloidal suspension of a hybrid nanomaterial system (HNMS). HNMS is a hybrid material system with designed amphiphilicity (hydrophilicity vs. hydrophobicity). Generally, the method includes dispersing nanomaterials (e.g., nanoparticles) having different shapes, sizes, and elemental compositions in water and sonicating the water with an ultrasonic probe to prepare the HNMS.
[0011] In a further embodiment, the present disclosure relates to a method for preparing a cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite. Generally, the method comprises: (1) dispersing carbon nanotubes (CNTs) in deionized water with CNCs to form a mixture; (2) sonicating the mixture; (3) immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-CNTs on the CF fabric; and (4) using vacuum assisted resin transfer molding (VaRTM) to manufacture the CNC-CNT-CF / epoxy hybrid composite.
[0012] In another embodiment, the present disclosure relates to a method for preparing a cellulose nanocrystal (CNC)-bound carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite. Generally, the method includes: (1) dispersing pristine carbon nanotubes (pCNTs) in deionized water with CNCs to form a mixture; (2) sonicating the mixture; (3) immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNTs on the CF fabric; and (4) using vacuum assisted resin transfer molding (VaRTM) to manufacture the CNC-CNT-CF / epoxy hybrid composite.
[0013] In another embodiment, the present disclosure relates to a method for preparing a cellulose nanocrystal (CNC)-bound carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite. Generally, the method includes: (1) dispersing functionalized CNTs (fCNTs) in deionized water with CNCs to form a mixture; (2) sonicating the mixture; (3) immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-fCNTs on the CF fabric; and (4) using vacuum assisted resin transfer molding (VaRTM) to manufacture the CNC-CNT-CF / epoxy hybrid composite.
[0014] In a further embodiment, the present disclosure relates to a method for preparing hybrid cellulose nanocrystals (CNC)-graphene nanosheets (boron nitride nanobarb) (GNP-(BNNB))-carbon fiber (CF) / polyetheretherketone (PEEK) using spraying. Generally, the method includes: (1) dispersing BNNB, CNC and GNP in deionized water to form a mixture; (2) treating CF / PEEK prepreg with plasma surface treatment; (3) coating the CF / PEEK prepreg with the mixture via a supercritical CO2-assisted atomization (SAA) system; and (4) forming the hybrid CNC-GNP (BNNB)-CF / PEEK via compression molding of the CF / PEEK prepreg.
[0015] In a further embodiment, the present disclosure relates to a method for preparing a cellulose nanocrystal (CNC)-bound carbon nanotube / graphene nanoplatelet carbon fiber reinforced polymer (CNT / GNP-CFRP) hybrid composite. Generally, the method comprises: (1) dispersing carbon nanotubes (CNT) and graphene nanoplatelets (GNP) in deionized water with CNC to form a mixture; (2) sonicating the mixture; (3) immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-CNT on the CF fabric; and (4) using vacuum assisted resin transfer molding (VaRTM) to manufacture the CNC-CNT / GNP-CF / epoxy hybrid composite.
[0016] In another embodiment, the present disclosure relates to a method for preparing a cellulose nanocrystal (CNC)-bound carbon nanotube / graphene nanoplatelet carbon fiber reinforced polymer (CNT-CFRP) hybrid composite. Generally, the method comprises: (1) dispersing pristine carbon nanotubes (pCNTs) and pristine graphene nanoplatelets (GNPs) in water with CNCs to form a mixture; (2) sonicating the mixture; (3) immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNTs on the CF fabric; and (4) using vacuum assisted resin transfer molding (VaRTM) to manufacture the CNC-CNT / GNP-CF / epoxy hybrid composite.
[0017] In further embodiments, the present disclosure is directed to a cellulose nanocrystal (CNC) bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition formed via the methods disclosed herein.
[0018] In additional embodiments, the present disclosure is directed to a cellulose nanocrystal (CNC) bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition formed via the methods disclosed herein.
[0019] In another embodiment, the present disclosure is directed to a cellulose nanocrystal (CNC) bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition formed via the methods disclosed herein.
[0020] In additional embodiments, the present disclosure relates to a hybrid cellulose nanocrystal (CNC)-graphene nanosheet (boron nitride nanobarb) (GNP-(BNNB))-carbon fiber (CF) / polyetheretherketone (PEEK) composition formed via the methods disclosed herein.
[0021] In a further embodiment, the present disclosure is directed to a cellulose nanocrystal (CNC) bonded carbon nanotube / graphene nanoplatelet carbon fiber reinforced polymer (CNT / GNP-CFRP) hybrid composite composition formed via the methods disclosed herein.
[0022] In additional embodiments, the present disclosure is directed to a cellulose nanocrystal (CNC) bonded carbon nanotube / graphene nanosheet carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition formed via the methods disclosed herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] A more complete understanding of the subject matter of the present disclosure may be obtained by referring to the following detailed description when taken in conjunction with the accompanying drawings, in which:
[0024] Figure 1 The zeta potential in water is illustrated (n:m indicates the mass ratio of constituent NM).
[0025] Figure 2 Illustrated are the water contact angles (WCA) of a pure water droplet on a membrane prepared with a hybrid nanomaterial system (HNMS).
[0026] Figure 3 Description of the in-house supercritical CO2-assisted atomization (SAA) system and optical diagnostic setup.
[0027] Figure 4 Illustrated are the Sauter mean diameter (SMD) of aqueous CNC droplets produced via SAA at 20 cm from the nozzle.
[0028] Figure 5 The pattern and cross-droplet height distribution of pattern vs. concentration SAA production are illustrated for 0.2, 0.5, 2 wt% aqueous CNCs in 3 μm droplets.
[0029] Figure 6 The cross-droplet height distribution of pattern vs. droplet diameter SAA production is illustrated for 2 wt% aqueous CNC and 3-11 μm droplet diameter.
[0030] Figure 7 State the sheet resistivity.
[0031] Fig. 8A Explain the binding energy between existing pairs of GNP-CNC.
[0032] Figure 8B The mean square displacement (MSD) is illustrated for (FIG. 8B1) GNP-CNC 12:1 and (FIG. 8B2) GNP-CNC 1:4.
[0033] Fig. 9 Comparison of AFM intermolecular forces and molecular dynamics (MD) total binding energy of GNP-CNC is illustrated.
[0034] Figures 10A-10C The mean square displacements of (FIG. 10A1, FIG. 10A2) CNC-GNP, (FIG. 10B1, FIG. 10B2) CNC-CNT and (FIG. 10C1, FIG. 10C2) CNC-BNNT pairs are illustrated. DETAILED DESCRIPTION
[0035] It should be understood that the following disclosure provides many different embodiments or examples for realizing the different features of various embodiments. The specific examples of parts and arrangements are described below to simplify the disclosure. Of course, these are merely examples and are not intended to be restrictive. The section headings used herein are for organizational purposes and should not be construed as limiting the subject matter described.
[0036] A novel spray deposition fabrication method is described herein, in which supercritical CO2-assisted atomization (SAA) is employed to fabricate three-dimensional (3D) multi-material nanostructures by depositing hybrid nanomaterial systems (HNMS) embedded in droplets of controlled size. Regardless of the shape and type of nanomaterial (NM), the degree of amphiphilicity of the HNMS and the ratio of the droplet diameter to the total mass of the HNMS within the droplet determine the balance of attractive, repulsive, and directional intermolecular forces between the HNMS, solvent, and substrate, which in turn determines the shape, size, and height of the resulting NM pattern. The following is elucidated herein: (1) the role of HNMS amphiphilicity on the molecular interactions between the HNMS, solvent, and substrate and the resulting intermolecular force balance; and (2) the role of droplet size and the mass of HNMS in the droplet on the intermolecular force balance, which determines the NM pattern during spray deposition. Three systems were used: (i) NMs of different types and geometries to construct HNMS; (ii) HNMS in different solvents and substrates; and (iii) aqueous droplets containing HNMS of different diameters and mass concentrations produced by SAA. To achieve these goals, the amphiphilicity of HNMS was characterized, and the evolution of intermolecular forces between HNMS, solvents and substrates during droplet evaporation was studied, and the effects of amphiphilicity and the properties of the sprayed droplets on these forces were elucidated using spectroscopy, laser diffraction and in situ atomic force microscopy (AFM). Cellulose nanocrystals (CNCs) were used as a platform for the degree of amphiphilicity of engineered HNMS. CNCs can be used to disperse and stabilize original carbonaceous nanoparticles, such as carbon nanotubes (pCNTs), graphene nanosheets (pGNPs), fullerenes, ceramic nanoparticles such as boron nitride nanotubes, nanobarbs and nanosheets, in proton media without functionalization. Here, the potential mechanism at the molecular level between the two that stabilizes the dispersion of CNCs and pCNTs / pGNPs in polar solvents was unraveled. Based on the characterization of CNC-pCNT / pGNP using spectroscopy and microscopy together with density functional theory (DFT) simulations, we propose that the main intermolecular mechanism between CNC and pCNT / pGNP is the formation of carbon-oxygen covalent bonds between hydroxyl groups on CNC and defects on pCNT / pGNP, leading to stabilization in polar solvents. These findings indicate that CNC-assisted processes enable new capabilities to exploit new structures at the molecular level and tailor the properties of nanocomposites at higher length scales.
[0037] Carbonaceous nanoparticles (such as carbon nanotubes (CNT) and GNP) have been widely used as fillers or as coatings on reinforcing fibers in polymer matrix composites (PMCs) to improve structure and electrical / thermal properties. Despite attempts to incorporate CNT / GNP into polymers and PMCs, such as melt / solution-mixing and in-situ polymerization, their mixtures are generally associated with CNT / GNP aggregation, poor interfacial interactions and degradation of intrinsic CNT / GNP properties. Although functionalization is effective for dispersing CNT / GNP, the method involves harsh chemical processes that damage CNT / GNP properties and limit process efficiency. Previous studies have shown that auxiliary nanoparticles make it possible for the aqueous dispersion of CNT / GNPs combined with nanomaterials such as graphene oxide (GO) rich in hydroxyl (-OH) groups and attached to the sidewalls. Cellulose nanocrystals (CNCs) make it possible for pGNPs and pCNTs to be stabilized in polar media without the need for functionalization. The uniqueness of CNCs is their ability to synergistically enhance the functionality of multi-material systems, such as optical / thermal management in electronic components and structural performance of various systems. Recent studies have demonstrated a new technique for CNC-assisted pCNT incorporation into carbon fiber reinforced polymers (CFRP) and its impact on mechanical properties. It was shown that CNCs not only do disperse and stabilize pCNTs in water, but also increase the flexural and interlaminar shear strength of CFRP due to the synergistic effect of pCNTs with CNCs.
[0038] In one embodiment of the claimed invention, molecular interactions between CNC and pCNT / pGNP are revealed, which lead to disassembly and stabilization in water. Both experimental and quantum level DFT simulations indicate that non-binding (physical) interactions between CNC and pCNT / pGNP cannot be the only mechanism for dispersing carbonaceous nanomaterials in water. Irreversible covalent bonds formed between CNC and defect sites on pCNT / pGNP are the main mechanism leading to disassembly and stabilization of carbonaceous nanoparticles in polar solvents.
[0039] Herein, a novel supercritical CO2-assisted spray method is described for fabricating three-dimensional multi-material nanostructured layouts by constructing NM patterns generated by depositing innovative building blocks (i.e., HNMS) embedded in aqueous droplets of controlled size. HNMS are multi-material systems composed of NMs of different shapes / sizes / types and opposite amphiphilic (hydrophilic vs. hydrophobic) properties combined in specific mass fractions. The results show that: (1) in supercritical CO2-assisted atomization (spray), CO2 is dissolved in water at a temperature and pressure above the thermodynamic critical point of CO2, enabling control of the size of droplets carrying HNMS; and (2) the shape and height of the spray-deposited pattern generated by HNMS aqueous droplets depend on the mass fraction of the NMs constituting the HNMS, the concentration of the HNMS, and the droplet size.
[0040] CNT (length l: 1.5 μm, and diameter d: 10 nm), GNP (l, width w: 2-5 μm, 6 nm thick) and BNNT (boron nitride nanotube) (l: 2 μm, d: 80 nm) were dispersed in CNC (d: 2.3-4.5 nm, l: 44-108 nm) + deionized water at various ratios at concentrations of 0.05-0.2 wt %, respectively, and probe sonicated for 2 h at 20 kHz and 75% amplitude. To study the HNMS in individual droplets and the formed NM patterns, six droplets of ~1.6 mm diameter were deposited on a glass substrate (micro cover glass No. 1.5) for each HNMS using a 0.1 μL Eppendorf pipette. The droplet evaporation time was ~16 min at 23 °C ± 0.1 and 50% humidity.
[0041] To investigate the hydrophobicity of HNMS, the water contact angle was measured using a goniometer by depositing a pure water droplet on the HNMS film. The HNMS film was prepared by depositing 1 mL of the prepared HNMS suspension on a Teflon membrane taped inside a Petri dish and drying at 80 °C for 4 h.
[0042] The effect of the mass fraction of the constituent NMs on the amphiphilicity of the HNMSs was investigated. CNCs effectively dispersed and stabilized hydrophobic pristine CNTs, GNPs, and BNNTs in water without the need for functionalization or the use of dispersants. In the absence of CNCs, the hydrophobic CNTs, GNPs, and BNNTs settled within a few minutes after stopping the ultrasonic treatment. Figure 1 The zeta potential of HNMS in water is shown (Malvern Zsizer). The higher the zeta potential value, the higher the hydrophilicity of the HNMS and the better the dispersion in water. Figure 1Indicating that changes in the mass ratio (fraction) of the constituent NMs alter the amphiphilicity of the HNMSs: increasing the CNC ratio increases the HNMS hydrophilicity because CNCs have abundant hydroxyl groups and negatively charged sulfate half-ester groups. As the hydrophobicity of the HNMSs increases, they are unstable in water and cannot be tested for zeta potential, so the water contact angle (WCA, ASTM D7334) was used to test and understand the relationship between the NM mass fraction and the hydrophobicity of the HNMSs by depositing pure water droplets on the HNMSs. Increasing the mass ratio of CNTs, GNPs, or BNNTs to CNCs in the HNMSs increased the WCA, indicating an increase in the hydrophobicity of the HNMSs ( Figure 2 ). These results suggest that changing the mass fraction of constituent NMs will alter the amphiphilicity of HNMSs regardless of the shape, size, and type of NMs.
[0043] Figure 3 A schematic diagram of the experimental setup with two high-pressure pumps for liquid and gas, a custom-designed high-pressure vessel, a 125 μm custom-made single-hole nozzle, and an optical diagnostic system is presented. The effects of the jet pressure, temperature, and CO2 concentration in the mixture on the droplet size have been fully characterized. The HNMS suspension is pumped into the high-pressure vessel, where it is mixed with high-pressure CO2. The pressurized ternary mixture (water-HNMS-CO2) is atomized into micron-sized droplets containing HNMS and deposited on a substrate at 25°C ± 0.1 and 50% humidity. A laser diffraction system (Malvern Panalytical's) captures the droplet diameters at different axial positions downstream of the nozzle.
[0044] Figure 4 Shown is the box plot distribution of the Sauter mean diameter (SMD; diameter of droplets with the same volume to surface area ratio) of aqueous CNCs (0.2 wt %) produced by SAA. Figure 4 It is revealed that the increase of CO2 pressure increases the solubility of CO2 in water and reduces the droplet size and narrows its distribution. The SMD has the smallest size and variation at and above supercritical pressures (7.5 and 9 MPa). These results show that the established SAA system can produce droplets containing HNMS with controlled size with a resolution of 2 ± 0.7 μm.
[0045] Figure 5 Shown are the height distributions of evaporated aqueous CNC droplets with a constant diameter of 3 μm and varying concentrations of 0.2, 0.5, and 2 wt. % produced by the SAA system on a glass substrate at 7.5 MPa. Figure 5 indicated that, at a constant droplet diameter, by increasing CNC concentration, the CNC pattern changed from rings to disks and domes, which is contrary to previous studies that reported that rod-shaped particles similar to CNCs tended to accumulate at the liquid-air interface. Figure 6 The height profiles for constant CNC concentration (2 wt%) and varying droplet diameters are compared and highlight that the pattern transitions from domes to rings by increasing the droplet size. Note that the Peclet (Pe) number, which is commonly used to describe the assembly of NMs in droplets by relating Brownian diffusion and evaporation-induced flows (advection) of NMs, cannot describe these patterns. For example, the Pe for 0.2 wt% and 0.5 wt% CNCs in 3 μm droplets are almost similar (0.33, 0.34), however, the patterns are different (rings vs. disks, Figure 5 ). For (i) different NM concentrations with constant droplet diameter and (ii) different droplet diameters with constant concentration ( Figures 5 and 6 ), the formation of different patterns of the same NMs implies that in addition to amphiphilicity, the ratio of droplet size to HNMS mass concentration is another key factor in NM patterning. This is addressed in Hypothesis 2.
[0046] Droplets of 3-5 μm containing GNP-CNC and CNT-CNC were spray-deposited at 7.5 MPa to cover 1 cm 2 Based on the results from the HNMS patterns generated after water evaporation, the HNMS amphiphilicity of GNP CNCs, CNT CNCs, and BNNT CNCs was compared with that from Figure 5 Based on the data from , the NM ratio and HNMS concentration were chosen to cover the substrate with either all rings or all disks after droplet evaporation. Figure 7 The four-point probe (Veeco FPP 500, NY, US) shown measures the sheet resistivity of the nanostructure. Pure original CNT and GNP are made into films for comparison. For GNP-CNC (1:4) and CNT-CNC (1:1) forming rings, in which conductive GNP and CNT are only present in the periphery, higher resistivity (lower conductivity) is recorded. By transferring to the disk, i.e. GNP-CNC (12:1) and CNT-CNC (5:1), the resistivity decreases as conductive NP covers the entire surface area. These results emphasize that the proposed spray deposition is capable of manufacturing multi-material nanostructures with desired functionality.
[0047] Fig. 8A The intermolecular forces between CNC and water, CNC and GNP, GNP and GNP, and GNP and water in the GNP-CNC system were resolved in water droplets at different ratios (12:1, 1:4). The binding energy between CNC and CNC in water is negligible because CNC is well dispersed and the interaction is long-range electrostatic repulsion (high zeta potential; Figure 1). A more negative value indicates a stronger binding. Comparison of GNP:CNC (12:1) with (1:4) shows that: (i) increasing the CNC ratio increases the binding energy of CNC and water, and increasing the GNP ratio increases the binding energy of GNP and GNP; and (ii) the interaction between CNC and GNP is very low. The main molecular interaction between CNC and water is hydrogen bonding (oriented), the main molecular interaction between GNP and GNP is van der Waals force (attraction), and the main molecular interaction between CNC and GNP is π bond (weak attraction). The weak binding energy between CNC and GNP indicates that the interaction between GNP and CNC from adjacent HNMS is minimal. Correlating the MD results with the HNMS amphiphilicity of the pattern vs. GNP CNC, CNT CNC and BNNT CNC in the HNMS pattern produced after water evaporation shows that the main intermolecular forces in patterning are van der Waals force (attraction), electrostatic repulsion (repulsion) and hydrogen bonding (oriented). Figure 8B The mean square displacement (MSD) is shown for ( FIG. 8B1 ) GNP-CNC 12:1 and ( FIG. 8B2 ) GNP-CNC 1:4.
[0048] Fig. 10B The movement of GNPs, CNCs, and water molecules over time was compared by measuring the mean square displacement values (MSD) of GNP:CNCs of 12:1 and 1:4. MSD is the cumulative displacement of particles over time. Comparison of the binding energy between existing pairs of GNP-CNC and MSD showed that when the GNP content was higher and the CNC content was lower (12:1 compared to 1:4), the MSD of GNPs was lower, which may be due to GNP aggregation and the MSD of water molecules was higher because they have more freedom to move. In contrast, when the GNP content was reduced and the CNC content was increased (4:1 compared to 12:1), more water molecules interacted with CNCs and the overall MSD of water molecules decreased. Interestingly, the MSD value of GNPs may increase because GNP aggregation is reduced due to the lower content. Although evaporation was not considered in the MD simulations, correlating the MSD and binding energy with the HNMS amphiphilicity of the patterns vs. GNP CNC, CNT CNC, and BNNT CNC in the HNMS patterns generated after water evaporation suggests that for GNP:CNC (12:1) during evaporation of the droplet, the formation of disks is more plausible than rings due to the slow movement of GNPs and CNCs and the aggregation of GNPs due to the high binding energy of GNPs and CNCs. In contrast, for GNP:CNC (1:4), the high binding energy of CNCs and water and the accelerated movement of CNCs and GNPs (towards the edge of the droplet during evaporation) imply the formation of rings, as shown in Figure 2 . Figure 6 What I see.
[0049] To verify the accuracy of the MD calculations, all binding energies were summed for a specific ratio and compared with the resulting AFM forces ( Fig. 9 ). The MD total binding energy of GNP-CNC(4:1) was 40% higher and the AFM intermolecular forces were 47% higher compared to GNP-CNC(12:1). Despite this agreement, the 7% discrepancy may be because the MD simulations did not consider the GNP-CNCs as unified HNMSs, in contrast to the AFM experiments. MD decomposes the individual forces; however, (i) the polarity of the substrate and solvent, (ii) the binding between the NMs constituting the HNMSs and their amphiphilicity, and (iii) the evaporation effect must be revealed to complete the general understanding.
[0050] Regardless of the shape and type of NMs, the degree of amphiphilicity of the HNMSs and the ratio of the droplet diameter to the total mass of HNMSs within the droplet determine the balance of attractive, repulsive, and directional intermolecular forces between the HNMSs, solvent, and substrate, which in turn determines the shape, size, and height of the resulting NM patterns.
[0051] The intermolecular forces of HNMS-solvent-substrate with various substrates (Al, SiO2, Si, PDMS) and solvents (water (PI: 10.1), ethanol (PI: 5.2) and toluene (~ non-polar)) will be characterized in a flow cell (MMTMEC Bruker, heater / cooler flow cell) in an AFM (AFM, Bruker Dimension Icon). Custom-made colloidal cantilever AFM probes with spherical tips (Si or Au 1-6.6 μm) are coated with HNMS. The spherical tip allows for uniform coating. In order to understand the intermolecular forces of HNMS-HNMS in solvents, substrates are coated with HNMS and the intermolecular forces are measured in different solvents. These measurements reveal how the interplay of HNMS amphiphilicity, solvent polarity and substrate surface energy controls the resulting intermolecular force balance.
[0052] The steps used to obtain nanoparticle suspensions are first the separation / disassembly of the nanoparticles, followed by stabilization. In the case of carbon nanoparticles (especially GNPs and CNTs), ultrasound treatment is used to induce disassembly, which can then be stabilized by CNC particles. To date, the dispersion mechanisms of CNFs and carbon nanomaterials have been explained by electrostatic interactions (in CNF-CNTs) and steric and hydrophobic interactions (in CNF-GNPs). These interactions are sufficient to stabilize CNT / GNPs with CNFs due to the higher aspect ratio and higher charge density of CNFs compared to CNCs. Therefore, the same dispersion mechanism may not be used for CNCs. Observations from basic molecular experiments and simulation studies suggest that in addition to physical interactions, another type of interaction must exist, namely chemical bonding: reactive sites on GNPs / CNTs, i.e., atoms surrounding their intrinsic defects, accommodate hydroxyl groups on CNCs and form bonds between the two structures. We assume that these bonds are irreversible and covalent and are one of the main mechanisms leading to stable disassembly of carbon nanoparticles in polar solvents.
[0053] To evaluate the effectiveness of the CNC in dispersing pCNTs in water, the dispersion quality of CNC-pristine CNTs (CNC-pCNTs) was compared with that of functionalized CNTs (e.g., CNC-weakly acid treated CNTs (CNC-fCNTs)) using UV-Vis spectroscopy. M CNT), CNT treated with strong acid and f H Since functionalization with strong acid treatment is a common method to increase the dispersibility of CNT / GNP in solvents (and especially in water), we functionalized CNT with sulfuric acid and compared their properties with pCNT. M The UV-Vis spectrum curve of CNT has a peak near 250 nm wavelength, which is consistent with previous studies of CNT aqueous suspensions. M The CNT curve shows two peaks at 223 nm (-OH groups) and 272 nm (graphite), indicating the presence of both CNCs and CNTs.
[0054] The stability of the dispersion mechanism was monitored for 21 days, during which time CNC-pCNT was stable. However, the CNC-pGNP suspension remained stable for only 2 days, which can be attributed to the insufficient number of CNCs attached to the micron-sized pGNPs. The CNFs were shown to be entangled on the graphene nanosheets, and the suspension was stable for three months. The steric hindrance and hydrophobic interactions between CNFs and GNPs promote the formation of an entangled network, and the highly charged carboxyl groups of CNFs provide strong electrostatic repulsion for a stable and uniform aqueous dispersion. The CNC-CNT / GNP interaction is in the form of physical interactions between the carbon bodies of the molecules and covalent bonds between defects on the CNT / GNPs and nucleophilic functional groups on the CNCs.
[0055] Construct multiple orientations of CNC to pCNT / pGNP to obtain the most stable energy configuration of the proposed combination. The potential reaction paths and Gibbs free energy values of three common carbon defects, i.e., single vacancy (sv), double vacancy (dv) and Stone-Wales (sw) were subsequently studied. Here, CNC was imitated with a dextran chain. A simulation involving a more practical model (a bundle of dextran chains) was also carried out, which returned similar results. Starting from a similar position, the reaction path involving a single vacancy defect ends the spontaneous reaction. The change in enthalpy is shown in the energy change of the thermodynamic system during the reaction, and its negative value is considered to be a sign of the favorableness of the reaction because it releases energy and is stable. The change in Gibbs free energy is another quantitative indication of the reaction, which includes both enthalpy and entropy changes between the initial and final states. Therefore, the falling pattern of both enthalpy and Gibbs free energy (both negative values) means that the reaction is theoretically barrier-free, and tilting means that the reaction requires input energy to occur. Here, the changes in both Gibbs free energy and enthalpy prove that single vacancy defects are feasible paths for CNC-svCNT reactions without energy barriers. However, CNC-svGNP reactions require a small amount of energy, which may be provided by ultrasonic treatment energy. Divacancy (Dv) and Stone-Wales (sw) defects are also more favorable than original conditions thermodynamically. Sw and perfect CNT / GNP produce absorbing energy reactions with CNC and water, while sv and dv prove more stable complexes in reaction path calculations. Overall results indicate that covalent bonding formation is possible for all types of defective CNT / GNPs with CNC.
[0056] Despite their similarities, the reaction paths of the pGNP system have different highlights compared to pCNTs in terms of both enthalpy and Gibbs energy. The transition state energy of the pGNP reaction path is much higher than that of the pCNTs. This can be attributed to the absence of bends that relieve the steric hindrance to the pCNTs. This is also responsible for the difference in the final energy state between CNC-pGNPs and CNC-pCNTs, which is about 30% lower in the case of CNC-pGNPs.
[0057] The binding status was also examined in the radial distribution factor (RDF). Here, the oxygen atoms on the CNCs were evaluated based on their distance from the carbon atoms of the pCNT / pGNP. Although the covalently bound carbon and oxygen atoms showed approx. The RDF value of C(pCNT)-O(CNC) is about It is very similar to similar chemical bonds. The resulting C(pCNT)-O(CNC) bond indicates that one of the carbon atoms on the periphery of the defect has been combined with one of the oxygen atoms on the CNC. The angle between the resulting CO bond and the pCNT surface is 109°. Single vacancy defects show higher reactivity, mainly due to the unsatisfied state of carbon. As a result of the CNC-pCNT combination, the chemical properties of the resulting hybrid system are slightly changed from non-polar pCNT to a more polar hybrid nanostructure, which indicates a trend of covalent bonding. The presence of the defect itself proves that there is no significant chemical change. Similar results are also observed for pGNP.
[0058] The reaction pathways calculated the energy required for covalent bonding between CNC and pGNP / pCNT, as well as their three types of defects. A CO bond was formed between one of the peripheral carbon atoms of the defect and the oxygen atom of the hydroxyl functional group of CNC. The results revealed the possibility of covalent bond formation, especially in the case of monovacancy defects. This suggests that the CNC-monovacancy interaction leads to spontaneous CO covalent bonding. The monovacancy bond energy in CNC-pCNT is 75 kcal / mol, which is comparable to 81.1 kcal / mol of the monovacancy bond in CNC-pGNP. Combined with the corresponding enthalpy and Gibbs free energy, the energy values show that the interactions between CNC-divacancy and CNC-Stone-Wales vacancy can be considered weaker compared to CNC-monovacancy, indicating that covalent bonding between CNC and the first two defects will form once the required energy is provided. This conclusion is also supported by comparing the corresponding bond lengths.
[0059] To verify the accuracy of the model system used in the DFT calculations, infrared (IR) spectra were calculated by DFT and compared with experimental FTIR results obtained from bulk CNC, CNC-pCNTs, and CNC-pGNPs. The agreement between the IR calculated and experimental FTIR spectra of cellulose monomers confirms that cellulose monomers and the theoretical level are reasonable models for CNCs. The results are in good agreement, for example, for all spectra (CNC and CNC-pCNT), the CH peak at 2905CM -1 Except for the OH stretching frequency at 3400CM -1 In addition, there is a small shift near 3410 cm between the experimental FTIR and DFT-calculated IR spectra of CNC-svCNT and unbound CNC-pCNT. -1Hydroxyl, ~2800CM -1 CH, ~1300CM -1 CH and ~1000CM -1 The samples were dried to remove the noise from the water and the peak at 1650 cm -1 The peak at 1063 cm corresponds to the water HOH bending mode, which is most likely due to the humidity in the air. The DFT calculated spectra of the unbound CNC-pCNT / pGNP and covalently bound CNC-svCNT / svGNP composites show similar trends to each other, with the two spectra matching at OH, CH, and CO. The oxygen-containing functional groups are expressed at 1063, 1264, and 1385 cm -1 The modeled CNC-svCNTs show bands at 1500 and 1000 cm -1 The experimental CNC-pCNTs have many peaks in this range, including C=C and CC groups, due to the available carbon sites of the unbound CNC-pCNTs. In addition, the pre-existing CO groups in the CNCs are indistinguishable from the newly formed covalent bonds in the experimental spectra. The calculated and experimental IR spectra do not distinguish between covalent bonding (CNC-svCNT / svGNP) and non-bonding interactions (CNC-pCNT / pGNP), but provide a general tool to verify the reliability of DFT calculations.
[0060] This work illustrates a new mechanism for stabilizing hydrophobic pCNT / pGNP in polar media by using CNCs without chemical functionalization or other additives. TEM micrographs show that CNCs approach pCNT / pGNPs in two ways: (1) side-by-side, resulting in non-binding physical interactions (e.g., van der Waals and C-π), and (2) from the tip to the side on the defective regions of CNT / GNPs. In these interactions, the shifts of XPS O1s in CNC-CNT / GNPs indicate that in addition to physical interactions, new C-O chemical bonds are formed between CNCs and pCNT / pGNPs. These bonds are in the form of covalent interactions between available hydroxyl and other oxygen-containing groups (e.g., sulfate groups) on CNCs and carbon atoms on the defect periphery on carbon nanoparticles.
[0061] Cellulose nanocrystals (CNCs) enable the efficient coating of carbon fibers with pristine carbon nanotubes (CNTs) and graphene nanosheets (GNPs). Here, we detail the mechanisms that form the interface of CNC-bound CNT and CNC-bound GNP-carbon fiber reinforced polymer (CFRP) composites. We show that CNCs provide a suitable platform to engineer the interface of hybrid composites. We demonstrate that hybrid nanomaterials (i.e., CNCs and CNT / GNPs) change the chemical composition of the interface and its properties, and that the mechanical properties of the produced composites are different despite the similar elemental composition of CNTs and GNPs. Our results show that the presence of CNC-CNTs and CNC-GNPs produces a 4 μm interfacial zone, which results in an increase of 200% and 145% in interfacial shear strength (IFSS), respectively, and an enhancement of 46% and 28% in interlaminar shear strength (ILSS). In addition, density functional theory (DFT) calculations show that the binding energy between CNC-CNTs and carbon fiber (CF) sizing agents is 14% higher than that of CNC-GNPs, which emphasizes the influence of chemical and physical interactions in the observed differences in mechanical properties. The understanding gained from this study highlights a pathway for bottom-up fabrication of hybrid composites with engineered microstructures and properties from the molecular level and nanoscale to higher scales.
[0062] Achieving desired properties from the self-assembly of nanoparticles is very challenging due to the complex nature of the interactions between the constituent building blocks. Self-assembly of nanocolloids by evaporation of particle-laden droplets can be exploited to fabricate tailored nanostructures that increase functionality and engineer the properties of the fabricated components. In this study, we used the unique amphiphilic properties of cellulose nanocrystals (CNCs) to prepare a hybrid system of graphene nanosheets (GNPs) and CNCs and engineered the architecture of the assembled nanostructures. We then employed a novel atomization system for high-throughput deposition of precisely controlled carrier droplets to form desired 3D patterns on a variety of substrates.
[0063] As one of the most critical aspects of nanotechnology, bottom-up nanofabrication methods have been extensively studied for building engineered 3D micro / nanostructures. Bottom-up techniques require some form of self-assembly of building blocks (e.g., atoms, molecules, and colloids) within a system that comes together to reach an equilibrium state and produce nanostructures with specific patterns (i.e., shape, size, thickness).
[0064] The supercritical CO2-assisted atomization (SAA) system described herein is capable of forming micron-sized carrier droplets with a narrow size distribution. The moderate operating conditions (i.e., temperature and pressure), low viscosity, high density and diffusivity, and high miscibility of CO2 in water and most organic solvents extend its compatibility with a variety of materials and promote its scalability as a viable option for large-scale deposition of NPs with desired properties on a variety of substrates. In addition, the system's sensitivity to slight changes in temperature and pressure allows the user to easily adjust the process parameters to achieve specific carrier droplet properties (e.g., size, flow rate, temperature, coverage) based on the requirements of the deposition application.
[0065] In one embodiment of the claimed invention, a nanoparticle-agnostic method is used that allows the manufacture of multi-material nanostructures with precisely engineered patterns. A novel spray atomization system is used to produce fine and uniform droplets as NP carriers to deposit 3D nanostructures with desired structures on different substrates. The functionality of these multi-material systems is also characterized, and different degrees of electrical properties are achieved by engineering the patterns of deposited nanoparticles. The developed system includes non-toxic, abundant and biocompatible reagents such as water, CNC and CO2, which promotes its scalability and adaptability.
[0066] The SAA system consists of two main feed lines, in which CO2 and injection suspension are pumped into a pressure vessel, and the ternary mixture (i.e., CO2, solvent and NP) stays to have enough time for the gas to dissolve in water. The temperature and pressure in the container are precisely controlled to remain at the critical point of CO2 (i.e., 31.5°C and 7.5MPa). The multiphase mixture is then injected into ambient pressure and temperature and injected toward the substrate of interest through a sprayer with a micron-sized injection hole (125 μm). The syringe is driven and controlled using an Arduino microcontroller system to operate at a resolution as low as 1 millisecond. The supercritical CO2 dissolved in the colloidal suspension forms bubbles, which expand and burst when injected into ambient temperature and pressure, which results in the fragmentation of the liquid jet and the formation of fine NP carrier droplets.
[0067] Template masking, a non-invasive method for controlling the deposition location, can be easily integrated with the SAA system. In SAA, masking combined with precise control over injection duration enables the shape and thickness of coatings to be engineered on any solid substrate.
[0068] MD simulations were further used to track the dynamics of the NPs and follow their movement in the water droplets over time (i.e., Brownian motion), which leads to the formation of specific patterns. Figure 10A-10CThe movement of NPs, CNCs and water molecules over time was compared by measuring the mean square displacement values (MSD) of HNMS with different degrees of amphiphilicity. MSD itself is the cumulative displacement of a particle over time. The MD model simulating CNC-NPs is a representative HNMS in a water droplet with a total of ~55,000 atoms (45K water atoms = 15K molecules) and a total of 10,000 atoms of CNCs and NPs with different ratios.
[0069] Comparing Figures 10A1-10C1 and Figures 10A2-10C2, it is shown that when the ratio of NP to CNC is high (i.e., HNMS dominated by hydrophobicity), the mobility of NP represented by the MSD value is low. This may be the result of NP aggregation. At the same time, water molecules show high mobility; this is because the aggregated phase is separated from the aqueous phase, severely limiting their interaction. This allows most water molecules to move unhindered. In contrast, when the ratio of NP to CNC decreases (i.e., HNMS dominated by hydrophilicity), the movement of water molecules is restricted, and CNC particles begin to move more freely in the droplets. This is due to the increase of water-CNC interactions, which attaches them to CNC molecules and greatly increases the mobility of CNC while limiting the movement of water molecules. Interestingly, in these hydrophilic dominant samples, the MSD values of NPs increase, which may be due to reduced NP aggregation. For example, comparing Figure 10A1 and Figure 10A2 at the 250 ps time scale shows that when the GNP content is higher and the CNC content is lower (12:1 compared to 1:4), the MSD of GNP and CNC is lower (compared to and Compared to and ), and the MSD of water molecules is higher (compared to Compared to
[0070] ). Although MD simulations do not take evaporation into account, correlating the MSD and interaction energies with the previous patterns suggests that for the predominantly hydrophobic HNMS in the evaporating droplet, the formation of disk-like patterns is more plausible than rings as the CNCs move slowly and the NPs aggregate due to the high NP-NP interaction energy. In contrast, for the predominantly hydrophilic samples, the high CNC-water interaction energy and the accelerated motion (i.e., high MSD values) of the CNCs and NPs (towards the edge of the evaporating droplet) indicate that the formation of ring-like patterns is more likely. It is worth emphasizing that the correlation of the interaction energy and motion of the particles with the final patterns they produce is independent of the size, shape, or material type of the NPs, and all CNC-bound GNP, CNT, and BNNT pairs follow the same trend in this regard.
[0071] The term "substantially" is defined as most but not necessarily all of the specified content, as understood by one of ordinary skill in the art. In any disclosed embodiment, the terms "substantially," "approximately," "substantially," and "about" may be replaced with "within [percentage] of the specified content," where percentages include 0.1, 1, 5, and 10%.
[0072] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art should understand that they can easily use the present disclosure as a basis to design or modify other processes and structures for carrying out the same purpose and / or realizing the same advantages of the embodiments introduced herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and they can make various changes, substitutions and modifications without departing from the spirit and scope of the present disclosure. The scope of the present invention should only be determined by the language of the appended claims. The term "comprising" in the claims is intended to mean "at least including" so that the list of elements listed in the claims is an open group. The terms "one", "an" and other singular terms are intended to include their plural forms unless explicitly excluded.
Claims
1. A method for depositing a nanostructure having an engineered pattern, the method comprising: selection of nanoparticles and substrates; and The nanoparticles are delivered to the substrate via a supercritical CO2-assisted atomization (SAA) system.
2. The method of claim 1, wherein the nanoparticles comprise one or more of: cellulose nanocrystals (CNC); two-dimensional or three-dimensional carbonaceous nanomaterials; carbon nanotubes (CNTs); graphene nanosheets (GNPs); fullerenes; ceramic nanoparticles; boron nitride nanobarb (BNNB), nanotubes (BNNTs) or nanosheets (BNNS); pristine CNTs (pCNTs); pristine GNTs (pGNTs); and combinations thereof. 3 . The method of claim 1 , wherein a three-dimensional (3D) nanostructure is formed by repeating the delivering step to form a pattern on the substrate.
4. The method of claim 4, wherein the pattern is generated and has a form selected from the group consisting of a ring, a disk, a dome, and combinations thereof.
5. The method of claim 1, wherein the nanoparticles comprise at least one of: first and second nanoparticles having different degrees of amphiphilicity to produce a desired pattern, CNC, GNP-CNC, CNT-CNC, or BNNT-CNC.
6. The method of claim 1, wherein the nanoparticles comprise at least one of: CNT-CNCs at a ratio of 1:1 to 1:10, GNP-CNCs at a ratio of 1:1 to 1:8, BNNT-CNCs at a ratio of 1:10 to 1:20, CNT-CNCs at a ratio of 5:1, GNP-CNCs at a ratio of 12:1 to 20:1, or BNNT-CNCs at a ratio of 1:
1. The method of claim 1 , wherein the nanoparticles comprise first nanoparticles and second nanoparticles.
8. The method of claim 7, wherein the first nanoparticles and the second nanoparticles have a ratio designed to produce an engineered amphiphilicity that is subsequently produced and patterned.
9. A method for preparing a colloidal suspension of a hybrid nanomaterial system (HNMS), wherein the HNMS comprises two or more nanomaterials connected by chemical and physical bonds, the method comprising: Nanomaterials of varying shapes, sizes, and elemental compositions are dispersed in water; and The water was sonicated with an ultrasonic probe to prepare the HNMS.
10. The method of claim 9, further comprising delivering the HNMS to a substrate via a supercritical CO2 assisted atomization (SAA) system.
11. The method of claim 10, further comprising repeating the delivering step to form a pattern on the substrate.
12. The method of claim 11, wherein the 3D nanostructures are produced by forming a pattern selected from the group consisting of rings, disks, domes, and combinations thereof.
13. The method of claim 11, wherein the pattern is produced by engineering the degree of amphiphilicity of the HNMS, which itself is designed by the ratio of different nanomaterials used in the HNMS.
14. The method of claim 9, wherein the substrate comprises at least one of glass, a polymer, a ceramic, or a semiconductor.
15. The method of claim 9, wherein the nanomaterial comprises one or more of: cellulose nanocrystals (CNC); two-dimensional or three-dimensional carbonaceous nanomaterials; carbon nanotubes (CNTs); graphene nanosheets (GNPs); fullerenes; ceramic nanoparticles; boron nitride nanobarbs (BNNBs), nanotubes (BNNTs) or nanosheets (BNNSs); pristine CNTs (pCNTs); pristine GNTs (pGNTs); and combinations thereof.
16. The method of claim 9, wherein the HNMS comprises at least one of GNP-CNC, CNT-CNC, or BNNT-CNC.
17. The method of claim 9, wherein the HNMS comprises at least one of: CNT-CNCs at a ratio of 1:1 to 1:10, GNP-CNCs at a ratio of 1:1 to 1:8, BNNT-CNCs at a ratio of 1:10 to 1:20, CNT-CNCs at a ratio of 5:1, GNP-CNCs at a ratio of 12:1 to 20:1, or BNNT-CNCs at a ratio of 1:
1.
18. The method of claim 9, wherein the nanomaterial comprises a first nanomaterial and at least a second nanomaterial.
19. The method of claim 18, wherein the first nanoparticles and the second nanoparticles have a ratio designed to produce an engineered amphiphilicity that is subsequently produced and patterned.
20. The method of claim 9, wherein the nanomaterial comprises at least one of weakly acid treated CNTs (fMCNTs), strongly acid treated CNTs (fHCNTs), CNC-fMCNTs, or CNC-fHCNTs.
21. The method of claim 20, wherein the fMCNTs or fHCNTs comprise CNTs treated with at least one of nitric acid or sulfuric acid.
22. A method for preparing a cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite material, the method comprising: dispersing carbon nanotubes (CNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the ultrasonically treated mixture in a bath sonicator to enhance the deposition of the CNC-CNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
23. The method of claim 22, wherein the CNTs are selected from the group consisting of weakly acid treated CNTs (fMCNTs), strongly acid treated CNTs (fHCNTs), pristine carbon nanotubes (pCNTs), and combinations thereof.
24. The method of claim 23, wherein the fMCNTs or fHCNTs comprise CNTs treated with at least one of nitric acid or sulfuric acid.
25. A method for preparing a cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite material, the method comprising: dispersing pristine carbon nanotubes (pCNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
26. A method for preparing a cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite material, the method comprising: dispersing functionalized CNTs (fCNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-fCNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
27. The method of claim 26, wherein the fCNTs comprise at least one of weakly acid treated CNTs (fMCNTs) or strongly acid treated CNTs (fHCNTs).
28. The method of claim 27, wherein at least one of the fMCNTs or fHCNTs comprises CNTs treated with at least one of nitric acid or sulfuric acid.
29. A method for preparing hybrid cellulose nanocrystal (CNC)-graphene nanosheet (boron nitride nanobarb) (GNP-(BNNB))-carbon fiber (CF) / polyetheretherketone (PEEK) using spraying, the method comprising: BNNB, CNC, and GNP were dispersed in deionized water to form a mixture; Treating CF / PEEK prepreg with plasma surface treatment; coating the CF / PEEK prepreg with the mixture via a supercritical CO2-assisted atomization (SAA) system; and The hybrid CNC-GNP(BNNB)-CF / PEEK was formed via compression molding of the CF / PEEK prepreg.
30. A method for preparing a cellulose nanocrystal (CNC)-bound carbon nanotube / graphene nanosheet carbon fiber reinforced polymer (CNT / GNP-CFRP) hybrid composite material, the method comprising: dispersing carbon nanotubes (CNTs) and graphene nanoplatelets (GNPs) in water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-CNT / GNPs on the CF fabric; and CNC-CNT / GNP-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
31. A method for preparing a cellulose nanocrystal (CNC)-bonded carbon nanotube / graphene nanosheet carbon fiber reinforced polymer (CNT-CFRP) hybrid composite material, the method comprising: pristine carbon nanotubes (pCNTs) and pristine graphene nanoplatelets (GNPs) are dispersed in water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNT / GNPs on the CF fabric; and CNC-CNT / GNP-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
32. A cellulose nanocrystal (CNC) bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition, wherein the composition is produced by a method comprising the steps of: dispersing carbon nanotubes (CNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the ultrasonically treated mixture in a bath sonicator to enhance the deposition of the CNC-CNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
33. A cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition, wherein the composition is produced by a method comprising the steps of: dispersing pristine carbon nanotubes (pCNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
34. A cellulose nanocrystal (CNC)-bonded carbon nanotube carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition, wherein the composition is produced by a method comprising the steps of: dispersing functionalized CNTs (fCNTs) in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-fCNTs on the CF fabric; and The CNC-CNT-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
35. A hybrid cellulose nanocrystal (CNC)-graphene nanosheet (boron nitride nanobarb) (GNP-(BNNB))-carbon fiber (CF) / polyetheretherketone (PEEK) composition, wherein the composition is produced by a method comprising the steps of: BNNB, CNC, and GNP were dispersed in deionized water to form a mixture; Treating CF / PEEK prepreg with plasma surface treatment; coating the CF / PEEK prepreg with the mixture via a supercritical CO2-assisted atomization (SAA) system; and The hybrid CNC-GNP(BNNB)-CF / PEEK was formed via compression molding of the CF / PEEK prepreg.
36. A cellulose nanocrystal (CNC)-bound carbon nanotube / graphene nanosheet carbon fiber reinforced polymer (CNT / GNP-CFRP) hybrid composite composition, wherein the composition is produced by a method comprising the steps of: dispersing carbon nanotubes (CNTs) and graphene nanoplatelets (GNPs) in water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-CNT / GNPs on the CF fabric; and CNC-CNT / GNP-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).
37. A cellulose nanocrystal (CNC)-bound carbon nanotube / graphene nanosheet carbon fiber reinforced polymer (CNT-CFRP) hybrid composite composition, wherein the composition is produced via a method comprising the steps of: pristine carbon nanotubes (pCNTs) and pristine graphene nanosheets (GNPs) were dispersed in deionized water with CNCs to form a mixture; sonicating the mixture; immersing a carbon fiber (CF) fabric together with the sonicated mixture in a bath sonicator to enhance the deposition of the CNC-pCNT / GNPs on the CF fabric; and CNC-CNT / GNP-CF / epoxy hybrid composites were fabricated using vacuum-assisted resin transfer molding (VaRTM).