Carbon fiber-containing concrete or mortar composition, carbon fiber-reinforced concrete or mortar structure, and method for producing same
By manufacturing a spindle-shaped carbon fiber aggregate and combining a binder, the problem of poor dispersion and handling of carbon fibers in concrete or mortar is solved, and efficient fiber reinforcement and excellent mechanical properties are achieved.
Patent Information
- Application Number
- CN202380029822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-12
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when carbon fibers are used as reinforcement materials in concrete or mortar structures, pre-cut short fibers or engineered scrap fibers are difficult to effectively utilize, and carbon fibers that have not been cured are easily dispersed into single fibers when combined with concrete, resulting in Reduced handling and bending toughness reinforcement are poor.
Using spindle-shaped carbon fiber aggregates, manufactured by rotary granulation or stir granulation, combined with binder to fix the fiber direction, ensure that the fiber bundle is not easy to loosen, and control the fiber length and binder content during the manufacturing process to form excellent and efficient fiber reinforcement effect.
It realizes efficient reinforcement using recycled carbon fiber, improves the bending strength and bending toughness of concrete or mortar structures, and ensures the handling and construction performance of the material.
Smart Images

Figure CN118973978A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a concrete or mortar composition containing a spindle-shaped carbon fiber aggregate, a reinforced concrete or mortar structure, and a method for producing the same. In particular, the present invention relates to a concrete or mortar composition containing a spindle-shaped carbon fiber aggregate made from recycled carbon fibers (recycled carbon fibers), a reinforced concrete or mortar structure, and a method for producing the same. Background Art
[0002] Concrete or mortar structures with cement as the main component are widely used in the fields of construction and civil engineering due to their excellent properties such as compressive strength, durability, and non-combustibility, as well as their low price. However, even when using aggregates such as sand and gravel, these structures are basically brittle and have the disadvantage of being easily cracked and damaged when subjected to tensile, bending, flexing, and other stresses.
[0003] Therefore, in order to compensate for these shortcomings, fiber-reinforced plastic wires (FRP wires) obtained by using steel fibers, synthetic fibers, aramid fibers, glass fibers, etc. are sometimes used as reinforcing materials in addition to the various aggregates that have been used. The mechanical properties of cement composite materials (reinforced concrete or mortar structures) such as bending strength and bending toughness are greatly improved.
[0004] Carbon fiber has excellent specific strength and specific elastic modulus, and is lightweight, so it is used as a reinforcing fiber for various materials. Furthermore, as a reinforcing fiber used in cement composite materials, it is also used in the fields of construction and civil engineering because it deteriorates less in alkali. In particular, various methods of using composite wires made of carbon fiber reinforced plastics (CFRP) obtained using carbon fibers as continuous fibers for cement composite materials have been studied.
[0005] For example, patent documents 1 to 3 describe cement composite materials made of composite wires, which are obtained by attaching a resin matrix or an inorganic matrix as an alternative to carbon fibers as continuous fibers, curing them, and cutting them. However, these methods are cut after curing the continuous fibers, and therefore cannot be applied to pre-cut short fibers, engineering scrap fibers, recycled carbon fibers from CFRP, etc. In addition, the manufacturing energy or cost of the curing process sometimes becomes a problem.
[0006] On the other hand, when pre-cut carbon fibers are used directly as reinforcing materials, they are not cured and are easily dispersed into single fibers when mixed with concrete compositions, etc. If dispersed into single fibers, the dispersed single fibers may be damaged due to contact with aggregates, and the viscosity of the material increases during mixing, which reduces the handling properties. In addition, there is a problem of reduced reinforcement effects such as bending toughness.
[0007] Patent Document 4 describes a cement composite material reinforced with carbon fibers having an average fiber length of 3 mm or less. Since the average fiber length is short, the probability of breakage of dispersed single fibers is low, but it is predicted that the reinforcement effect of the flexural strength, flexural toughness, etc. of the obtained cement composite material is small. In addition, since the material viscosity increases, the slump and fluidity, which are characteristic values of the mortar composition before curing, decrease.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent No. 5046276
[0011] Patent Document 2: Japanese Patent No. 5054906
[0012] Patent Document 3: Japanese Patent No. 5182779
[0013] Patent Document 4: Japanese Patent No. 5809019 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The purpose of the present disclosure is to provide a reinforcing material using pre-cut carbon fibers such as short fibers, engineering scrap fibers, recycled carbon fibers recovered from CFRP, etc. as raw materials, to make a concrete or mortar composition containing carbon fibers with excellent handleability, and to provide a carbon fiber reinforced concrete or mortar structure with a high fiber reinforcement effect as its cured product.
[0016] Another object of the present disclosure is to provide a method for producing a carbon fiber reinforced concrete or mortar structure.
[0017] Means for solving problems
[0018] According to the following aspects of the present invention, the above-mentioned problems can be solved:
[0019] <Method 1>
[0020] A concrete or mortar composition containing carbon fibers, characterized in that it comprises a carbon fiber aggregate consisting of at least carbon fibers and a binder.
[0021] The carbon fiber aggregate has a spindle shape.
[0022] <Method 2>
[0023] The carbon fiber-containing concrete or mortar composition according to Embodiment 1, wherein the average length of the spindle-shaped carbon fiber aggregate is 1.5 mm to 60 mm.
[0024] <Method 3>
[0025] The carbon fiber-containing concrete or mortar composition according to aspect 1 or 2, wherein the average maximum width of the spindle-shaped carbon fiber aggregate is 0.1 mm to 3.0 mm.
[0026] <Method 4>
[0027] The carbon fiber-containing concrete or mortar composition according to any one of aspects 1 to 3, wherein the average length of the carbon fibers is 1 mm or more and less than 30 mm.
[0028] <Method 5>
[0029] The carbon fiber-containing concrete or mortar composition according to Embodiment 4, wherein the average length of the carbon fiber aggregate is 1.2 to 5.0 times the average length of the carbon fibers contained in the carbon fiber aggregate.
[0030] <Method 6>
[0031] The carbon fiber-containing concrete or mortar composition according to any one of aspects 1 to 5, wherein the content of the binder is 0.1 to 10% by weight relative to the spindle-shaped carbon fiber aggregate.
[0032] <Method 7>
[0033] The carbon fiber-containing concrete or mortar composition according to any one of aspects 1 to 6, wherein the carbon fiber includes regenerated carbon fiber.
[0034] <Method 8>
[0035] The carbon fiber-containing concrete or mortar composition according to any one of aspects 1 to 7, wherein the carbon fiber is regenerated carbon fiber.
[0036] <Method 9>
[0037] The carbon fiber-containing concrete or mortar composition according to Embodiment 7 or 8, wherein the regenerated carbon fiber contains a residual carbon component, and the residual carbon component is more than 0 wt % and not more than 5.0 wt % relative to the regenerated carbon fiber.
[0038] <Method 10>
[0039] A carbon fiber reinforced concrete or mortar structure obtained by curing the composition according to any one of aspects 1 to 9.
[0040] <Method 11>
[0041] A method for producing a carbon fiber reinforced concrete or mortar structure comprises producing a spindle-shaped carbon fiber aggregate composed of at least carbon fibers and a binder.
[0042] <Method 12>
[0043] The method according to embodiment 11, wherein the carbon fiber comprises recycled carbon fiber.
[0044] <Method 13>
[0045] The method according to embodiment 11 or 12, wherein the carbon fiber is recycled carbon fiber.
[0046] <Method 14>
[0047] The method according to method 12 or 13 includes: decomposing the plastic components contained in the plastic product containing carbon fibers by a semiconductor thermal activation method to produce the aforementioned regenerated carbon fibers.
[0048] Effects of the Invention
[0049] According to the present invention, a carbon fiber-containing concrete or mortar composition having excellent handleability can be provided by using a reinforcing material using pre-cut carbon fibers such as short fibers, engineering scrap fibers, recycled carbon fibers recovered from CFRP, etc. as raw materials, and a carbon fiber-reinforced concrete or mortar structure having a high fiber reinforcement effect as its cured product, and a method for manufacturing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 is a schematic diagram of one embodiment of an agitator granulator that may be used in the present disclosure.
[0051] Figure 2 This is a photograph of a plurality of carbon fiber aggregates of Example 1.
[0052] Figure 3 This is a photograph of a carbon fiber aggregate of Example 1.
[0053] Figure 4 This is a photograph of a plurality of carbon fiber aggregates of Example 2. DETAILED DESCRIPTION
[0054] The concrete or mortar composition disclosed in the present disclosure is characterized in that it contains at least a carbon fiber aggregate composed of at least carbon fibers and a binder, and contains a spindle-shaped carbon fiber aggregate.
[0055] The concrete or mortar composition disclosed in the present disclosure contains a spindle-shaped carbon fiber aggregate. Although not intended to be limited by theory, the spindle-shaped carbon fiber aggregate can be manufactured by a rotation granulation method, a stirring granulation method, etc., so it can be considered that the carbon fiber is subjected to stress in a certain direction such as centrifugal force, so that the single fibers are arranged in a certain direction and bundled, and are firmly fixed by a binder. Therefore, it can be considered that when mixing with a concrete composition, the bundle is not easy to loosen, and it can be suppressed from dispersing into single fibers.
[0056] In addition, the concrete or mortar structure disclosed in the present invention is preferably reinforced with a spindle-shaped carbon fiber aggregate having an average length of 1.5 mm to 60 mm. The spindle-shaped carbon fiber aggregate is characterized in that even if the length of the pre-cut carbon fiber that serves as the raw material is less than 1.5 mm, it can be extended in terms of the average length of the carbon fiber aggregate. Therefore, as a reinforcing material, it is possible to increase the fixing force with the concrete structure, etc., and therefore, for tensile stress, the reinforcing material is not easily removed from the concrete structure, etc. that serves as the base material, and good reinforcement efficiency can be obtained.
[0057] That is, the present disclosure has found that a spindle-shaped carbon fiber aggregate has excellent properties as a reinforcing material for concrete structures and the like using pre-cut carbon fibers as a raw material, and thus provides a cement composite material having a high fiber reinforcement effect.
[0058] Hereinafter, the invention of the present disclosure will be described in further detail.
[0059] <Carbon Fiber Aggregate>
[0060] The carbon fiber aggregate described in the present disclosure is an aggregate composed of at least carbon fibers and a binder. In the carbon fiber aggregate, single fibers are bonded to each other by the binder.
[0061] The amount of the binder in the carbon fiber aggregate is preferably 0.1 to 10% by weight, particularly preferably 0.5 to 8% by weight or 1 to 6% by weight relative to the carbon fiber aggregate. When the amount of the binder is less than 0.1% by weight, the bundles are easily loosened and dispersed into single fibers when kneaded with a concrete composition, etc., and the single fibers are sometimes broken, and the viscosity of the material during kneading increases, which reduces the handleability, so it is not preferred.
[0062] When the amount of the binder exceeds 10% by weight, the weight ratio of the carbon fibers constituting the carbon fiber aggregate becomes small, so that when compared with the same addition amount of the aggregate, there is a tendency that good reinforcement efficiency cannot be obtained.
[0063] The carbon fiber aggregate described in the present disclosure has a spindle shape. It should be noted that the spindle shape refers to a shape that is thick in the middle and gradually becomes thinner toward both ends.
[0064] As a particularly preferred embodiment of the method disclosed herein, a method for obtaining a spindle-shaped carbon fiber aggregate using a stirring granulation method is described in detail below. As a similar method, a method for obtaining a spindle-shaped carbon fiber aggregate using a rotating granulation method can be referred to, for example, the description of Japanese Patent No. 3452363.
[0065] (Average length of the aggregate)
[0066] The average length of the carbon fiber aggregate can be 1.5 mm to 60 mm. The average length of the aggregate is preferably 5 mm or more, 10 mm or more, 15 mm or more, 20 mm or more, or 25 mm or more, and / or preferably 55 mm or less, 50 mm or less, 45 mm or less, or 40 mm or less. When the average length of the carbon fiber aggregate is less than 1.5 mm, the fixing force with the concrete structure is small, and the aggregate is easily removed from the concrete structure as the base material for tensile stress, and good reinforcement efficiency cannot be obtained, so it is not preferred.
[0067] When the average length of the carbon fiber aggregate exceeds 60 mm, it may be difficult to uniformly mix the aggregate into a concrete composition, etc. In addition, since the aggregates are entangled with each other during kneading, it may be difficult to further uniformly disperse them into a concrete composition, etc.
[0068] The average length of the carbon fiber aggregate can be calculated by measuring the lengths of 50 carbon fiber aggregates in the long axis direction visually with a caliper or in an image obtained with a digital camera or an optical microscope, and averaging the measured values.
[0069] The average length of the carbon fiber aggregate is preferably 1.2 to 5.0 times the average length of the carbon fibers contained in the carbon fiber aggregate. When the average length of the carbon fiber aggregate is within the above range, good reinforcement efficiency may be obtained.
[0070] The average length of the carbon fiber aggregate is particularly preferably 1.4 times or more, 1.5 times or more, or 1.6 times or more of the average length of the carbon fibers, and / or, particularly preferably 4.5 times or less, 4.0 times or less, 3.5 times or less, 3.0 times or less, or 2.5 times or less. When the average length of the carbon fiber aggregate is within the above range, particularly good reinforcement efficiency can sometimes be obtained.
[0071] (Average maximum width of the aggregate)
[0072] The average maximum width of the carbon fiber aggregate can be 0.1mm to 3.0mm. The average length of the aggregate is preferably 0.2mm or more, 0.3mm or more, 0.4mm or more, or 0.5mm or more, and / or preferably 2.8mm or less, 2.6mm or less, 2.4mm or less, 2.2mm or less, or 2.0mm or less. The average maximum width of the carbon fiber aggregate is the maximum average length (width) in a direction perpendicular to the length direction. When the average maximum width of the carbon fiber aggregate is less than 0.1mm, the aggregate sometimes breaks, and the fixing force with the concrete structure is small and the short aggregate becomes more, and a good reinforcement efficiency cannot be obtained, so it is not preferred.
[0073] In addition, if the average maximum width of the carbon fiber aggregate is greater than 3.0 mm, the number of aggregates dispersed in the concrete structure etc. decreases when the same addition amount of the aggregate is compared. As a result, there is a tendency that the total contact surface area with the concrete structure etc. becomes smaller and good reinforcement efficiency cannot be obtained.
[0074] The average maximum width of the carbon fiber aggregate can be calculated by measuring the lengths of 50 carbon fiber aggregates in the minor axis direction visually with a caliper or in an image obtained with a digital camera or an optical microscope, and averaging the measured values.
[0075] (Aspect Ratio)
[0076] The aspect ratio of the aggregate can be 5 to 150. The aspect ratio of the aggregate is preferably 10 or more, 15 or more, 20 or more, 25 or more, or 30 or more, and / or 120 or less, 100 or less, 80 or less, or 60 or less. The aspect ratio of the carbon fiber aggregate is the value obtained by dividing the major diameter of the spindle-shaped aggregate by the minor diameter, and can be set as the average length / average maximum width. As the degree of slenderness increases, the aspect ratio increases. When the aspect ratio is less than 5, the total surface area in contact with the concrete structure, etc. becomes smaller, and the fixing force becomes smaller, so it is not preferred that a good reinforcement efficiency cannot be obtained.
[0077] When the aspect ratio is larger than 150, it is difficult to uniformly mix into a concrete composition or the like, and the aggregate may break, so that good reinforcement efficiency tends not to be obtained.
[0078] (Carbon Fiber)
[0079] Carbon fiber is a raw material of the aggregate, and examples thereof include ordinary carbon fiber (carbon fiber that is not recycled carbon fiber, so-called virgin carbon fiber), recycled carbon fiber, and mixtures thereof. The carbon fiber may be, for example, PAN-based carbon fiber or pitch-based carbon fiber.
[0080] The form of the carbon fiber is not particularly limited, and may be in the form of a carbon fiber bundle composed of a plurality of monofilaments (filaments). The number of filaments constituting the carbon fiber bundle may be in the range of 1,000 to 80,000 or 3,000 to 50,000. In addition, the diameter of the filaments constituting the carbon fiber may be 0.1 μm to 30 μm, 1 μm to 10 μm, or 3 μm to 8 μm.
[0081] (Recycled Carbon Fiber)
[0082] Recycled carbon fiber (recycled carbon fiber) contains carbon fiber components and carbon components other than the carbon fiber components (particularly residual carbon components). Generally, in the recycled carbon fiber, the carbon components other than the carbon fiber components adhere to the surface of the carbon fiber components.
[0083] The regenerated carbon fiber is not particularly limited, and may be, for example, regenerated carbon fiber obtained by heat-treating a plastic product containing carbon fiber, such as carbon fiber reinforced plastic (CFRP).
[0084] The regenerated carbon fiber is particularly preferably a regenerated carbon fiber obtained by a semiconductor thermal activation method. A particularly preferred embodiment of the method described below includes: decomposing a plastic component contained in a plastic product containing carbon fiber by a semiconductor thermal activation method to produce the regenerated carbon fiber.
[0085] It should be noted that the "thermal activation of semiconductors" (TASC method) is a method of decomposing decomposable compounds such as polymers by utilizing the thermal activation of semiconductors (TASC). For the method of manufacturing recycled carbon fibers by decomposing the plastic components contained in plastic products containing carbon fibers by the semiconductor thermal activation method, reference can be made to, for example, the records of Japanese Patent No. 4517146 and Japanese Patent Gazette No. 2019-189674.
[0086] The carbon fiber component in the regenerated carbon fiber may be modified by being subjected to heat treatment during the production process of the regenerated carbon fiber, etc. For details of the carbon fiber component in the regenerated carbon fiber, reference may be made to the above-mentioned description of the carbon fiber.
[0087] The residual carbon component in the recycled carbon fiber usually originates from the resin contained in the carbon fiber-containing plastic product used as a raw material when manufacturing the recycled carbon fiber. Generally speaking, during the heat treatment of the carbon fiber-containing plastic product, the plastic component undergoes thermal decomposition, and the residual carbon remains on the surface of the carbon fiber component.
[0088] In the present disclosure, the residual carbon content is preferably more than 0% by weight and 5.0% by weight or less relative to the regenerated carbon fibers. In this case, an aggregate with improved reinforcement efficiency may be obtained.
[0089] Although not intended to be limited by theory, it is believed that when the residual carbon content exceeds 0 wt% and is 5.0 wt% or less, the carbon content (especially carbon) that may become foreign matter that prevents the single fibers from being arranged and bundled in a certain direction when the spindle-shaped carbon fiber aggregate is manufactured is reduced. Therefore, an aggregate that is firmly fixed by a binder can be obtained, and it is believed that the bundle is not easily loosened when kneading with a concrete composition, etc., and dispersion into single fibers can be suppressed.
[0090] The residual carbon content is preferably 4.0% by weight or less, 3.0% by weight or less, or 2.0% by weight or less relative to the regenerated carbon fiber. The residual carbon content is preferably as low as possible and may be 0.1% by weight or more, 0.2% by weight or more, 0.4% by weight or more, 0.6% by weight or more, 0.8% by weight or more, 1.0% by weight or more, or 1.2% by weight or more relative to the carbon fiber.
[0091] The content of the residual carbon component in the regenerated carbon fiber can be measured by thermogravimetric analysis (TGA method).
[0092] The residual carbon content can be measured by thermogravimetric analysis as follows:
[0093] (i) A 1 to 4 mg sample piece obtained by pulverizing the regenerated carbon fiber was subjected to a thermogravimetric analysis in a thermogravimetric analyzer for a total of about 600 minutes at an air supply rate of 0.2 L / min, a heating rate of 5°C / min, and a recording rate of 1 / 6 s, with the following steps:
[0094] From room temperature to 100°C,
[0095] Keep at 100℃ for 30 minutes.
[0096] From 100°C to 400°C, and
[0097] Maintain at 400°C for 480 minutes;
[0098] (ii) In a graph in which the weight reduction rate is plotted against time, the inflection point of the slope is determined, and the weight reduction rate during the holding period at 100° C. is subtracted from the value of the weight reduction rate at the inflection point to calculate the residual carbon amount.
[0099] When the inflection point of the slope cannot be determined under the above conditions, the temperature may be maintained at a specific temperature within a range of more than 400° C. and 500° C. or less for 480 minutes instead of maintaining at 400° C. for 480 minutes.
[0100] When the regenerated carbon fiber has a resin derived from a sizing agent or the like, the above measurement may be performed after removing the resin.
[0101] (Average length of carbon fiber)
[0102] The carbon fibers may have an average length of 1 mm or more and less than 30 mm. Fibers having a length in this range may be obtained, for example, by cutting fibers having a longer size. The average length of the carbon fibers may be 2 mm or more, 3 mm or more, or 4 mm or more, and / or may be 29 mm or less, 28 mm or less, 27 mm or less, 26 mm or less, 25 mm or less, 24 mm or less, 23 mm or less, 22 mm or less, 21 mm or less, or 20 mm or less. In particular, the average length of the carbon fibers may be 8 mm to 25 mm or 9 mm to 20 mm.
[0103] It can be considered that when the average length of the carbon fiber is 1 mm or more and less than 30 mm, the single fibers are arranged and bundled in a certain direction, and the bundles are not easy to loosen when mixed with concrete compositions, etc., and the dispersion into single fibers can be suppressed. Although it does not mean to be limited by theory, it can be considered that by making the average length of the fibers used as raw materials sufficiently long, the fibers are easily oriented in one direction, and a spindle-shaped aggregate can be obtained. In addition, it can be considered that by making the average length of the fibers sufficiently short, the fibers are prevented from being entangled with each other, and the uniform orientation of the fibers is promoted.
[0104] The average length of the carbon fibers can be calculated by measuring the lengths of 50 carbon fibers visually using a caliper or the like or in an image obtained using a digital camera or an optical microscope or the like, and averaging the measured values.
[0105] 《Method for producing spindle-shaped carbon fiber aggregate》
[0106] The method for producing a spindle-shaped carbon fiber aggregate disclosed in the present invention comprises the following steps:
[0107] Providing a mixture consisting of at least carbon fibers and a liquid containing a binder (providing step);
[0108] Producing a spindle-shaped precursor by rotating the mixture in a container (granulation step); and
[0109] The precursor is dried (drying step).
[0110] Regarding the respective components described in the above-mentioned production method, reference can be made to the above-mentioned description on the assembly of the present disclosure.
[0111] <Providing process>
[0112] In the method disclosed in the present disclosure, a mixture consisting of at least carbon fibers and a liquid containing a binder is provided. The mixture particularly comprises carbon fibers and a solution containing a binder.
[0113] The amount of the liquid containing the binder in the mixture is preferably 10% to 70% by weight, particularly preferably 15% to 60% by weight or 20% to 50% by weight. In this case, the fibers are particularly well bundled due to the liquid contained in the binder. In addition, in this case, the burden of the drying process can be reduced because the amount of liquid contained in the binder is not excessive.
[0114] (Liquid containing binder)
[0115] The liquid containing the binder is a binder dispersion or a binder solution, which contains a binder and a solvent or a dispersion medium.
[0116] (Binder)
[0117] The binder has the effect of bundling the carbon fibers in the aggregate and maintaining the shape of the aggregate. The binder is not particularly limited, and is preferably a thermoplastic resin or a thermosetting resin. More specifically, as the binder, epoxy resin, urethane-modified epoxy resin, vinyl ester resin, acrylic resin, polyester resin, phenolic resin, polyamide resin, polyurethane resin, polycarbonate resin, polyetherimide resin, polyamideimide resin, polyimide resin, bismaleimide resin, polysulfone resin, polyethersulfone resin, epoxy-modified urethane resin, polyvinyl alcohol resin, polyvinyl pyrrolidone resin can be listed. These resins can be used alone or in combination of two or more.
[0118] In addition, as binders, bentonite, lignin sulfonate, syrup, carboxymethyl cellulose, konjac powder, sodium alginate, polyacrylamide, polyvinyl acetate, polyvinyl alcohol, and starch can also be listed. These can be used alone or in combination of two or more, and can also be used in combination with the above-mentioned resins.
[0119] (Solvent, dispersion medium)
[0120] The solvent or dispersion medium is not particularly limited as long as it is a liquid that can dissolve or disperse the binder. Examples of the solvent or dispersion medium include water, alcohol (e.g., methanol or ethanol), ketone (e.g., methyl ethyl ketone or acetone), hydrocarbon (e.g., cyclohexane, toluene or xylene), halogenated hydrocarbon (e.g., dichloromethane), amide (e.g., N-methylpyrrolidone or dimethylformamide), and ether (e.g., tetrahydrofuran). The solvent or dispersion medium is particularly preferably water.
[0121] The liquid containing the binder used in the present disclosure can be prepared by, for example, further adding a solvent or a dispersion medium to a commercially available sizing agent having a higher concentration of the binder and the solvent or the dispersion medium. In particular, the liquid containing the binder can be prepared by adding a dispersion medium (especially water) to a sizing agent having a binder and a dispersion medium (especially water).
[0122] The sizing agent (and a liquid containing a binder obtained by adding a solvent or a dispersion medium to the sizing agent) may be in the form of an aqueous emulsion in which the binder is dispersed in water, for example, and may be a water-based polyurethane in particular.
[0123] The concentration of the binder in the sizing agent is not particularly limited, and may be, for example, 10 to 80% by weight, 20 to 60% by weight, or 30 to 50% by weight.
[0124] The amount of the binder may be 0.5% by weight or more, 1% by weight or more, 1.5% by weight or more, 2.0% by weight or more, or 3.0% by weight relative to the liquid containing the binder, and / or may be 20% by weight or less, 18% by weight or less, 16% by weight or less, 14% by weight or less, or 12% by weight or less. The amount of the binder is particularly preferably 1% to 16% by weight or 2% to 12% by weight relative to the liquid containing the binder.
[0125] The amount of the binder is preferably 0.1 to 10% by weight, particularly preferably 0.5 to 8% by weight or 1 to 6% by weight, based on the carbon fiber aggregate.
[0126] (Fiber opening)
[0127] The fiber components, especially the carbon fibers, may be subjected to a fiber opening treatment in advance. The fiber opening treatment may eliminate the entanglement between the fibers and promote the orientation of the fibers in one direction in the granulation step.
[0128] The carbon fibers that can be used to produce the spindle-shaped carbon fiber aggregate may be subjected to a fiber opening treatment in advance. The fiber opening treatment may promote the alignment and bundling of the single fibers in a certain direction in the pelletizing step.
[0129] The method of the fiber opening treatment is not particularly limited, and the fiber opening treatment can be performed using, for example, a rotary blade. The rotary blade used for fiber opening can be an auxiliary blade installed in a pelletizer.
[0130] In addition, the fiber opening treatment can also be carried out by high-speed stirring.
[0131] (mix)
[0132] In the method for producing a spindle-shaped carbon fiber aggregate, the method for obtaining a mixture from carbon fibers and a liquid containing a binder is not particularly limited. The carbon fibers and the liquid containing a binder can be put into a container used in a granulation process in the form of a mixture. For example, a mixture is obtained by injecting a liquid containing a binder into a block of carbon fibers and stirring it at will, and the mixture is put into a container. Alternatively, the carbon fibers and the liquid containing a binder can be put into a container separately, and mixed in the container to form a mixture. Mixing and granulation can be performed simultaneously.
[0133] The carbon fibers and the liquid containing the binder in the mixture do not necessarily need to be uniformly distributed in the mixture. The mixture can be stirred during the pelletizing process to improve uniformity.
[0134] <Granulation process>
[0135] In the method for producing a spindle-shaped carbon fiber aggregate according to the present disclosure, a spindle-shaped precursor is produced by tumbling a mixture in a container (hereinafter, this process may also be referred to as "granulation process").
[0136] The method for tumbling the mixture in the container is not particularly limited, and a known method (particularly a known granulation method) can be used.
[0137] In particular, the spindle-shaped precursor is manufactured by rotating the mixture in the container in the gap between the inner wall of the container and the rotating body in the container. Although not intending to be limited by theory, it is believed that by rotating the mixture containing carbon fibers and the liquid containing the binder in the gap between the inner wall of the container and the rotating body in the container, the fibers are oriented in a specific direction and bonded to each other by the binder, and as a result, a precursor having a spindle shape can be obtained particularly effectively.
[0138] The method for rotating the mixture in the gap between the inner wall of the container and the rotating body in the container is not particularly limited. Figure 1 The following description is given.
[0139] Figure 1 is a schematic diagram of one embodiment of an agitator granulator that can be used in the present disclosure. Figure 1 The stirring granulator 10 includes a cylindrical container portion 12 as a container and a stirring blade 14 as a rotating body. Figure 1 The stirring granulator 10 is of a horizontal type, and in a normal use state, the opening of the container portion 12 opens toward the side. Figure 1 The diagram is viewed from the perspective of looking into the interior of the container. A shaft 16 is mounted on the inner wall of the container 12 (the inner wall in the above perspective) opposite to the opening. The shaft 16 extends in the horizontal direction. The stirring blade 14 can rotate (in the direction of rotation) with the shaft 16 as the center. Figure 1 In the example shown, the rotation is counterclockwise ("A"), but it can be clockwise. Figure 1 The stirring blade 14 is configured to rotate in a plane parallel to the gravity direction. Figure 1 Although not shown, auxiliary blades for opening the fibers may be provided in the container portion 12 .
[0140] In the granulation process, the mixture containing the carbon fiber and the liquid containing the binder is randomly mixed and stirred by the stirring blade 14 rotating in the container part 12, and the inner wall of the container part 12 and the stirring blade 14 in the container part 12 (at Figure 1 The device rotates within the gap (indicated by the symbol "C" in the figure).
[0141] The granulation treatment may be performed at ambient temperature or by heating. The granulation treatment may be performed for, for example, 1 minute to 1 hour, 5 minutes to 20 minutes, or 8 minutes to 15 minutes.
[0142] (container)
[0143] The container disclosed herein is not particularly limited as long as it is suitable for holding the mixture therein and subjecting the mixture to the above-mentioned granulation treatment. The container is preferably formed of a material having excellent rigidity and durability. It is particularly preferred that the inner wall of the container is formed of a material that does not cause abrasion when the mixture is rotated or is surface-treated for this purpose.
[0144] In one embodiment of the present disclosure, the container is not tilted and is substantially parallel to the horizontal direction. For example, the portion of the inner wall of the container located at the bottom in the gravity direction is not tilted and can be substantially parallel to the horizontal direction.
[0145] (rotating body)
[0146] The rotating body is configured such that, by rotating in the container, a mixture containing carbon fibers and a liquid containing a binder can be rotated between the rotating body and the inner wall of the container. The rotating body is mounted on, for example, a shaft provided in the container and is configured to be rotatable around the shaft.
[0147] The rotating body preferably has the form of a blade (paddle). The rotating body is particularly preferably a stirring blade (stirring blade). The stirring blade is preferably formed of a material having excellent rigidity and durability, and is particularly preferably formed of a material that does not wear out when the mixture rotates or has been surface treated for this purpose.
[0148] (gap)
[0149] The size of the gap between the inner wall of the container and the rotating body, that is, the distance between the inner wall of the container and the rotating body may be constant, or may be various values that are continuous or discontinuous.
[0150] The size of the gap between the inner wall of the container and the rotating body in the container, that is, the distance between the inner wall of the container and the rotating body can be appropriately set according to the desired size of the carbon fiber aggregate, and can be, for example, 1 to 10 mm.
[0151] (Mixing Granulator)
[0152] As the device having the above-mentioned container and the rotating body, a known stirring granulator can be used. The stirring granulator is not particularly limited, and for example, a Henschel type granulator (Henschel mixer), a mud kneader type granulator or an EIRICH type stirring granulator can be used. The stirring granulator can be either vertical or horizontal.
[0153] (Spindle-shaped precursor)
[0154] The spindle-shaped precursor contains carbon fibers and a binder, and contains liquid (especially water) derived from the liquid containing the binder. The liquid (especially water) in the precursor can be removed by the following drying process.
[0155] <Drying process>
[0156] In the method for producing a spindle-shaped carbon fiber aggregate according to the present disclosure, the obtained spindle-shaped precursor is dried.
[0157] The method for drying the precursor is not particularly limited, and the temperature conditions, time conditions, and the like can be appropriately determined according to the moisture content of the obtained precursor and the like.
[0158] 《Concrete or mortar composition containing carbon fiber》
[0159] The mortar composition disclosed in the present disclosure is obtained by adding water to spindle-shaped carbon fiber aggregates, cement, sand and other fine aggregates, and mixed materials and kneading them. The concrete composition is obtained by kneading coarse aggregates such as gravel on the basis of these raw materials. Various additives, other raw materials, etc. can be mixed into such concrete or mortar compositions for the purpose of improving physical properties in accordance with the application.
[0160] <Carbon Fiber Addition Rate>
[0161] The addition rate (content) of the carbon fibers constituting the spindle-shaped carbon fiber aggregate described in the present disclosure can be selected according to the application, and is preferably 0.01 to 10 volume % relative to the total amount of the concrete or mortar composition, and can be 0.05 to 5 volume %, 0.1 to 3 volume % or 0.2 to 1.5 volume %. Furthermore, the spindle-shaped carbon fiber aggregate described in the present disclosure can be used in combination with an existing reinforcing fiber material. When the addition rate of carbon fibers is less than 0.01 volume %, good reinforcement efficiency cannot be obtained, so it is not preferred.
[0162] In addition, when the addition rate of carbon fiber exceeds 10 volume %, it is sometimes difficult to uniformly mix the aggregate into the concrete composition, etc. In addition, since the aggregates are entangled with each other during kneading, it is sometimes difficult to further uniformly disperse them into the concrete composition, etc. In addition, the viscosity of the concrete composition, etc., sometimes increases, and the handling property decreases, which is not preferred.
[0163] <Method of adding carbon fiber aggregate>
[0164] As a method for adding the spindle-shaped carbon fiber aggregate described in the present disclosure to a concrete composition, etc., there are, for example, the following methods: a method in which cement, fine aggregate, coarse aggregate, etc. are pre-dry-premixed with the aggregate, and water is added and kneaded; or a method in which cement, fine aggregate, coarse aggregate, etc. are fully stirred with water, and then the aggregate is added and kneaded.
[0165] As a stirrer for kneading, a pan stirrer, a tilting stirrer, an omnimixer, a Hobart mixer, a truck stirrer, or the like can be used.
[0166] <<Carbon Fiber Reinforced Concrete or Mortar Structures>>
[0167] The concrete or mortar structure disclosed in the present invention can be manufactured by solidifying the above-mentioned concrete or mortar composition obtained by the above operation. In these structures, the carbon fiber can exist in the state of the spindle-shaped carbon fiber aggregate described in the present invention, or a part or all of the aggregate can be loosely bundled and dispersed into single fibers or fiber bundles. In the manufacturing method of these structures, by using the carbon fiber aggregate for kneading with a concrete composition, etc., even if it is dispersed into single fibers or fiber bundles during manufacturing, a structure with less breakage and uniform dispersion of carbon fibers can be obtained.
[0168] The method for curing the concrete or mortar composition is not particularly limited, and the curing method and conditions thereof can be appropriately determined according to the type of structure, construction conditions, layout conditions, environmental conditions, etc. It can be used for construction methods and repair methods such as 3D printing, covering, injection, filling, masonry work, and blowing.
[0169] Example
[0170] Hereinafter, the present invention will be described in more detail using examples. It should be noted that the examples are for illustration only and the present application is not limited thereto.
[0171] 《Example 1》
[0172] <Material Preparation>
[0173] (Carbon Fiber)
[0174] As the carbon fiber, regenerated carbon fiber obtained by a semiconductor thermal activation method and having an average single fiber diameter of 6.7 μm, a single fiber tensile strength of 5.3 GPa, a Weibull shape factor of 7.6, and a residual carbon content of 1.4 wt % was used.
[0175] (Single fiber tensile strength)
[0176] The single fiber tensile strength was measured according to JIS R7606 as follows:
[0177] Take at least 30 single fibers from the fiber bundle,
[0178] The diameter of the single fiber was measured in the side image of the single fiber taken by digital microscopy, and the cross-sectional area was calculated.
[0179] The sampled single fibers are fixed to the open-cell backing paper using an adhesive.
[0180] The liner paper with the single fiber fixed was installed in a tensile testing machine, and a tensile test was performed under the conditions of a test length of 10 mm and a deformation speed of 1 mm / min to measure the tensile breaking stress.
[0181] The tensile strength is calculated based on the cross-sectional area and tensile breaking stress of a single fiber.
[0182] The average value of the tensile strengths of at least 30 single fibers was taken as the single fiber tensile strength.
[0183] (Weibull shape coefficient)
[0184] The Weibull shape factor is calculated as follows:
[0185] lnln{1 / (1-F)}=m×lnσ+C
[0186] (Where F is the failure probability obtained by the symmetrical specimen cumulative distribution method, σ is the single fiber tensile strength (MPa), m is the Weibull shape coefficient, and C is a constant.)
[0187] Weibull plotting was performed using lnln{1 / (1-F)} and lnσ, and the Weibull shape coefficient m was calculated from the slope obtained by the first-order fitting.
[0188] (Residual carbon content)
[0189] The amount of residual carbon content in the regenerated carbon fiber was determined by thermogravimetric analysis (TGA method) as follows:
[0190] (i) A 4 mg sample piece obtained by pulverizing regenerated carbon fiber was subjected to thermogravimetric analysis for a total of about 600 minutes at an air supply rate of 0.2 L / min, a heating rate of 5° C. / min, and a recording rate of 1 / 6 s in a thermogravimetric analyzer, the thermogravimetric analysis having the following steps:
[0191] Heating from room temperature to 100°C, holding at 100°C for 30 minutes, heating from 100°C to 400°C, and holding at 400°C for 480 minutes;
[0192] (ii) In a graph in which the weight reduction rate is plotted against time, the inflection point of the slope is determined, and the weight reduction rate during the holding period at 100° C. is subtracted from the value of the weight reduction rate at the inflection point to calculate the amount of residual carbon.
[0193] (Average length of carbon fiber)
[0194] Recycled carbon fibers cut to an average length of 15 mm were used.
[0195] (Liquid containing binder)
[0196] A binder-containing liquid (aqueous emulsion sizing agent) having 255 g of water as a dispersion medium relative to 10.2 g of a urethane resin as a binder was prepared.
[0197] (Granulation treatment)
[0198] For the granulation treatment, a vertical stirring granulator (30 L MTI stirrer, manufactured by Tsukishima Machinery Co., Ltd.) was used.
[0199] The stirring granulator has stirring blades and also has auxiliary blades for promoting fiber opening.
[0200] As the stirring blades began to rotate, 500 g of the above-mentioned regenerated carbon fibers and 265 g of the above-mentioned liquid containing the binder were added to the container portion of the stirring granulator, and mixed and granulated for 10 minutes at the ambient temperature to obtain a spindle-shaped precursor.
[0201] The water content of the mixture was 33.3% by weight. The rotation speed of the stirring blade was 290 rpm, and the rotation speed of the auxiliary blade was 5,000 rpm.
[0202] (Drying treatment)
[0203] The obtained precursor was dried in a dryer to obtain the carbon fiber aggregate described in Example 1.
[0204] (Collective)
[0205] Figure 2 and Figure 3These are photographs of the carbon fibrous agglomerate described in Example 1. As can be seen in these figures, the carbon fibrous agglomerate described in Example 1 has a spindle-like shape.
[0206] (Binder content)
[0207] The content of the binder in Example 1 was 2.0% by weight relative to the aggregate.
[0208] (average length and average maximum width)
[0209] When measured with a caliper with 50 specimens (N=50), the average length of the carbon fiber aggregate described in Example 1 was 32.8 mm and the average maximum width was 0.9 mm. The average length of the regenerated carbon fiber was 15 mm, so the average length of the carbon fiber aggregate was 2.2 times the average length of the regenerated carbon fiber.
[0210] (Aspect Ratio)
[0211] The aspect ratio (long diameter / short diameter) of the aggregate of Example 1 was calculated. The long diameter is the length of the aggregate, and the short diameter is the maximum width of the aggregate. The average value was calculated for 50 specimens (N=50) based on the above measured values, and the aspect ratio was 36.
[0212] <Manufacturing of Mortar Composition Containing Carbon Fiber>
[0213] (Preparation of raw mortar composition)
[0214] Using a mortar mixer (5L MIC-362, manufactured by Marui Co., Ltd.), 9.0 g of the carbon fiber aggregate of Example 1 was mixed with 1265 g of low-heat silicate cement (manufactured by Pacific Seminto Co., Ltd.), 569 g of fine aggregate (No. 6 silica sand, manufactured by Sanyo Silicone Co., Ltd.), 4.5 g of a mixing agent (water reducing agent Master Glenium SP8HU, manufactured by BASF) and 380 g of water at a stirring speed of 140 rpm for about 3 minutes.
[0215] The addition rate of carbon fibers in the obtained raw mortar composition was 0.5% by volume, the water / cement ratio was 30.0% by weight, and the fine aggregate / cement ratio was 45.0% by weight.
[0216] (Bundling of carbon fibers after mixing)
[0217] A small amount of raw mortar composition was taken out and washed with water, and the extracted carbon fiber aggregate was visually observed. When the spindle-shaped carbon fiber aggregate was maintained and cement was not observed to penetrate between the monofilaments, the bundling was considered to be good. On the other hand, when the bundling was loose and the aggregates observed to penetrate between the monofilaments accounted for more than 10% by weight of the whole, the bundling was considered to be poor. The results are shown in Table 1 below.
[0218] (Flowability of raw mortar composition)
[0219] A flow cone (a conical column with a height of 6 cm, an inner diameter of 10 cm on the lower surface, and an inner diameter of 7 cm on the upper surface, which is hollowed out on the inner side) is placed on a horizontally arranged 50 cm square aluminum plate, and the raw mortar composition is injected to make it flat, and the flow cone is slowly pulled vertically upward. When the diameter of the raw mortar composition expanded into a circle on the aluminum plate or the circle is deformed, the arithmetic average of the shortest diameter and the longest diameter is measured as the flow value. The flow value reflects the fluidity of the raw mortar composition, and a raw mortar composition with a high flow value tends to be able to obtain good molding construction properties. The results are shown in the following Table 1.
[0220] <Manufacturing of Carbon Fiber Reinforced Mortar Structure>
[0221] The raw mortar composition of Example 1 was poured into a mold frame of width 40 mm×height 40 mm×length 160 mm, cured in air at 20°C for 2 days, and then cured in water at 20°C for 4 days to produce a mortar structure specimen (cured product) for bending failure energy measurement.
[0222] For the obtained test piece, three-point bending measurement was performed according to JIS R5201. In more detail, a universal material testing machine (A&D Co., Ltd., TENSILON universal material testing machine RTF2410) was used to compress the center of the 10 cm distance between the fulcrums at a speed of 2 mm / min. In addition, the bending strength was calculated from the obtained maximum bending stress. In addition, the area under the bending stress-load point displacement curve obtained until the load point displacement was 4 mm was calculated as the bending failure energy. The results are shown in Table 1 below.
[0223] 《Example 2>>
[0224] <Material Preparation>
[0225] (Carbon Fiber)
[0226] Regenerated carbon fibers were used in the same manner as in Example 1 except that the carbon fibers were cut to an average length of 10 mm.
[0227] (Liquid containing binder)
[0228] A binder-containing liquid (aqueous emulsion sizing agent) having 291 g of water as a dispersion medium relative to 10.2 g of a urethane-based resin as a binder was prepared.
[0229] <Granulation treatment>
[0230] For the granulation treatment, a vertical stirring granulator (20 L Loedige mixer, manufactured by Mathbo Co., Ltd.) was used.
[0231] The stirring granulator has stirring blades and also has auxiliary blades for promoting fiber opening.
[0232] As the stirring blades began to rotate, 500 g of the above-mentioned regenerated carbon fibers and 301 g of the above-mentioned liquid containing the binder were added to the container portion of the stirring granulator, and mixed and granulated for 10 minutes at the ambient temperature to obtain a spindle-shaped precursor.
[0233] The water content of the mixture was 36.3% by weight. The rotation speed of the stirring blade was 320 rpm, and the rotation speed of the auxiliary blade was 3,000 rpm.
[0234] (Drying treatment)
[0235] The obtained precursor was dried in a dryer to obtain the carbon fiber aggregate described in Example 2.
[0236] (Collective)
[0237] Figure 4 This is a photograph of the carbon fiber aggregate described in Example 2. The obtained carbon fiber aggregate has a spindle shape.
[0238] (Binder content)
[0239] The content of the binder in Example 2 was 2.0% by weight relative to the aggregate.
[0240] (average length and average maximum width)
[0241] The average length of the carbon fiber aggregate evaluated in the same manner as in Example 1 was 18.9 mm and the average maximum width was 1.6 mm. Since the average length of the regenerated carbon fibers was 10 mm, the average length of the carbon fiber aggregate was 1.9 times the average length of the regenerated carbon fibers.
[0242] (Aspect Ratio)
[0243] The aspect ratio evaluated in the same manner as in Example 1 was 12 based on the above measured values.
[0244] <Manufacturing of Mortar Composition Containing Carbon Fiber and Carbon Fiber Reinforced Mortar Structure>
[0245] A raw mortar composition and a mortar structure were prepared and evaluated in the same manner as in Example 1, except that the carbon fiber aggregate described in Example 2 was used instead of the carbon fiber aggregate described in Example 1. The results are shown in Table 1 below.
[0246] Comparative Example 1>>
[0247] In Comparative Example 1, the raw mortar composition and mortar structure were produced and evaluated in the same manner as in Example 1, except that a raw carbon fiber bundle (24,000 single fibers per bundle, an average single fiber diameter of 6.8 μm, a single fiber tensile strength of 5.4 GPa, and a Weibull shape factor of 4.9) cut to an average length of 10 mm was used instead of the aggregate of the regenerated carbon fibers. The results are shown in Table 1 below.
[0248] <<Reference Example 1>>
[0249] A raw mortar composition and a mortar structure were prepared and evaluated in the same manner as in Example 1 except that carbon fiber was not added and fiber reinforcement was not performed. The results are shown in Table 1 below.
[0250] The raw mortar compositions of Examples 1 and 2 show the same fluidity as the raw mortar composition of Reference Example 1 that is not fiber-reinforced, and show better fluidity than the raw mortar composition of Comparative Example 1. The reasons for this are as follows: the carbon fiber aggregates of Examples 1 and 2 have a higher bundling force than the cut original carbon fiber bundles of Comparative Example 1, which inhibits their dispersion into single fibers, and therefore the viscosity of the raw mortar composition does not increase. In addition, the mortar structures of Examples 1 and 2 have higher bending strength and bending failure energy than the mortar structure of Reference Example 1 that is not fiber-reinforced. Therefore, by using the raw mortar compositions of Examples 1 and 2, excellent molding workability and reinforcement efficiency can be obtained at the same time.
[0251] In addition, the mortar structure of Example 1 has a further increased bending strength and bending failure energy compared to the mortar structure of Example 2, and despite containing recycled carbon fibers, still shows a higher bending strength and bending failure energy than the mortar structure of Comparative Example 1. Although not intended to be limited by theory, the reasons for this can be listed as follows: the carbon fiber aggregate of Example 1 has a longer average length than the aggregate of Example 2, and the fixing force with the mortar is further increased, so the aggregate is more difficult to be removed from the mortar with respect to tensile stress, and the reinforcement efficiency is particularly good.
[0252] [Table 1]
[0253]
[0254] Description of Reference Numerals
[0255] 10 Mixing Granulator
[0256] 12 Container
[0257] 14 Mixing blade
[0258] 16 Shaft
[0259] A Rotation direction
[0260] C Clearance
Claims
1. A concrete or mortar composition containing carbon fibers, It is characterized in that The invention comprises a carbon fiber aggregate composed of at least carbon fibers and a binder. The carbon fiber aggregate has a spindle shape.
2. The carbon fiber-containing concrete or mortar composition according to claim 1, in, The average length of the carbon fiber aggregate is 1.5 mm to 60 mm.
3. The carbon fiber-containing concrete or mortar composition according to claim 1 or 2, in, The average maximum width of the carbon fiber aggregate is 0.1 mm to 3.0 mm.
4. The carbon fiber-containing concrete or mortar composition according to claim 1 or 2, in, The average length of the carbon fibers is greater than or equal to 1 mm and less than 30 mm.
5. The concrete or mortar composition containing carbon fibers according to claim 4, in, The average length of the carbon fiber aggregate is 1.2 to 5.0 times the average length of the carbon fibers contained in the carbon fiber aggregate.
6. The carbon fiber-containing concrete or mortar composition according to claim 1 or 2, in, The content of the binder is 0.1 to 10 wt % based on the spindle-shaped carbon fiber aggregate.
7. The carbon fiber-containing concrete or mortar composition according to claim 1 or 2, in, The carbon fibers include recycled carbon fibers.
8. The concrete or mortar composition containing carbon fibers according to claim 7, in, The carbon fiber is recycled carbon fiber.
9. The concrete or mortar composition containing carbon fibers according to claim 7, in, The regenerated carbon fiber includes a residual carbon component, and the residual carbon component is more than 0 weight % and 5.0 weight % or less relative to the regenerated carbon fiber.
10. A carbon fiber reinforced concrete or mortar structure obtained by curing the composition according to claim 1 or 2.
11. A method for producing a carbon fiber reinforced concrete or mortar structure, wherein include: A spindle-shaped carbon fiber aggregate composed of at least carbon fibers and a binder is produced.
12. The method according to claim 11, in, The carbon fibers include recycled carbon fibers.
13. The method according to claim 12, in, The carbon fiber is recycled carbon fiber.
14. The method according to claim 12 or 13, wherein include: The regenerated carbon fiber is produced by decomposing plastic components contained in a plastic product containing carbon fiber through a semiconductor thermal activation method.
Citation Information
Cited By
Regenerated fiber reinforced sulphoaluminate cement-based ultra-high performance concrete for retired wind turbine blade and preparation method of regenerated fiber reinforced sulphoaluminate cement-based ultra-high performance concrete
CN122277197A
A recycled fiber reinforced sulphoaluminate cement-based ultra-high performance concrete from decommissioned wind turbine blades and a method of making the same
CN122277197B