Polymer brominated flame retardant, composition with polymer brominated flame retardant and cable with polymer brominated flame retardant

By using tetrabromophthalic anhydride diamine siloxane and silane functionalized polyolefin compositions in polymers, the flame retardant properties and thermal stability of brominated flame retardant in polyolefin systems are solved. Good flame retardant effect and low toxicity characteristics are achieved.

CN118974121APending Publication Date: 2024-11-15DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280091918.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing brominated flame retardants have problems with high environmental durability, bioaccumulativeness and toxicity in polymers, and have poor flame retardant performance in polyolefin systems, making it difficult to meet the strictest combustion performance requirements and thermal stability requirements. .

Method used

Using tetrabromophthalic anhydride diamine siloxane as flame retardant, the reaction of amino functionalized siloxane with tetrabromophthalic anhydride to generate heat-stable aromatic bromide, combined with silane-functionalized polyolefins , a polymer composition that is easily dispersed is formed, and the flame retardant performance is improved.

Benefits of technology

It achieves good flame retardant properties in polyolefin systems, reduces concerns about bioaccumulation and toxicity characteristics, enhances carbon formation capabilities, improves compatibility of different polarities, and meets the strictest combustion performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974121A_ABST
    Figure CN118974121A_ABST
Patent Text Reader

Abstract

The invention provides tetrabromo phthalic anhydride diamine siloxane, and a preparation method of the tetrabromo phthalic anhydride diamine siloxane. In one embodiment, there is provided a tetrabromophthalic anhydride diamine siloxane (TDS) having a structural formula (1) # imgabs0 # wherein n is an integer from 1 to 40; and each R is the same or different, and each R is independently selected from the group consisting of hydrogen and a C1-C20 hydrocarbyl group. The present disclosure also provides a polymer composition comprising the TDS of Formula (1) and a cable comprising the TDS of Formula (1).
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Polymer compositions containing halogenated flame retardants are known. One category of halogenated flame retardants is the category of brominated flame retardants. Brominated flame retardants are able to meet the most stringent combustion performance requirements. However, a disadvantage of many brominated flame retardants is that they are toxic. Brominated flame retardants such as decabromodiphenylethane, decabromodiphenyl ether, tetrabromobisphenol A bis(2,3-dibromopropyl) ether and ethylene bistetrabromophthalimide are known to have high environmental persistence, bioaccumulation and toxicity (PBT).

[0002] There is a growing interest in one type of brominated flame retardants, polymeric brominated flame retardants or "PBFRs". Unlike conventional brominated flame retardants - PBFRs have reduced PBT properties because PBFRs do not easily penetrate biological systems due to their large size. The two main types of PBFRs are brominated styrene-ethylene-butylene-styrene (SEBS) and brominated polystyrene. Brominated SEBS is not thermally stable because the Br is attached to the alkyl groups of the SEBS. There will be a premature dissociation of the C-Br bond. In brominated polystyrene, the Br is attached to the aromatic ring, which is stable during compounding and processing. However, due to poor compatibility with polyolefins, brominated SEBS does not perform well in flame retardant properties in polyolefin based systems.

[0003] There is a recognized need in the art for polymeric brominated flame retardants that are capable of meeting the most stringent flame performance requirements while also exhibiting low potential for bioaccumulation and toxicity characteristics and suitable thermal stability to withstand melt blending and / or extrusion with polyolefins. Summary of the invention

[0004] The present disclosure provides a tetrabromophthalic anhydride diamine siloxane. In one embodiment, a tetrabromophthalic anhydride diamine siloxane (TDS) is provided, wherein the TDS has a structure of formula (1):

[0005] Formula (1)

[0006]

[0007] wherein n is an integer from 1 to 40; and

[0008] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.

[0009] The present disclosure provides a polymer composition. In one embodiment, a polymer composition is provided, and the polymer composition contains a flame retardant, and the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1):

[0010] Formula (1)

[0011]

[0012] wherein n is an integer from 1 to 40; and

[0013] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 In a further embodiment, the polymer composition comprises a silane-functionalized polyolefin.

[0014] The composition of the present invention includes an article. In one embodiment, the article is a cable and includes a conductor and a coating on the conductor. The coating comprises a silane-functionalized polyolefin; and a flame retardant. The flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1):

[0015] Formula (1)

[0016]

[0017] wherein n is an integer from 1 to 40; and

[0018] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20

[0019] A group consisting of hydrocarbon groups.

[0020] The inventors functionalized tetrabromophthalic anhydride with amino-functionalized siloxane to produce a heat-stable aromatic bromide based on a phthalimide siloxane structure. The brominated phthalimide structure provides a stable aromatic bromide during processing and effective bromide release, and the stable aromatic bromide shows excellent flame retardant performance. The siloxane unit provides a suitable molecular weight to reduce biological penetration, reduce PBT concerns about bioaccumulation and toxicity characteristics, and increase carbon formation. In addition, the incorporated siloxane unit improves the compatibility of components with different polarities through its flexibility and low surface energy characteristics. Therefore, compared to other polymer brominated flame retardants, the tetrabromophthalic anhydride diamine siloxane of the present invention is easily dispersed in a polymer matrix. The tetrabromophthalic anhydride diamine siloxane of the present invention shows good flame retardancy in a polyolefin-based system.

[0021] Figure 1 is a tetrabromophthalic anhydride diamine siloxane (TDS) according to one embodiment of the present disclosure 1 H-NMR spectrum.

[0022] Figure 2 According to one embodiment of the present disclosure Figure 1TDS 13 C-NMR spectrum.

[0023] Figure 3 According to one embodiment of the present disclosure Figure 1 FT-IR spectrum of TDS.

[0024] definition

[0025] Any reference to the Periodic Table of the Elements is to the Periodic Table as published by CRC Press, Inc., 1990-1991. A group of elements in this table is referred to by a new notation for numbering the groups.

[0026] For purposes of U.S. patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or their equivalent U.S. versions are incorporated by reference), particularly with respect to disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure).

[0027] The numerical range disclosed herein includes all values ​​from the lower limit to the upper limit, and includes the lower limit and the upper limit. For a range containing clear values ​​(e.g., 1 or 2, or 3 to 5, or 6, or 7), any sub-range between any two clear values ​​is included (e.g., the above range 1 to 7 includes 1 to 2; 2 to 6; 5 to 7; 3 to 7; 5 to 6; etc.).

[0028] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are based on weight and all test methods are current as of the filing date of this disclosure.

[0029] "Alkyl group" is a saturated straight chain, cyclic or branched hydrocarbon group. Non-limiting examples of suitable alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl (or 2-methylpropyl) and the like.

[0030] An "aminoalkyl group" is an alkyl group containing one or more amino groups.

[0031] An "amino group" is a nitrogen atom attached to a hydrogen atom and / or a hydrocarbon by a single bond.

[0032] The term "blend" or "polymer blend" as used refers to a mixture of two or more polymers. A blend may be miscible or immiscible (not phase separated at the molecular level). A blend may or may not be phase separated. A blend may or may not contain one or more domain configurations, as determined by transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art. A blend may be achieved by physically mixing two or more polymers at a macroscopic level (e.g., melt blending resins or compounding) or a microscopic level (e.g., simultaneously formed in the same reactor).

[0033] The term "composition" refers to a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0034] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not these components, steps or procedures are specifically disclosed. For the avoidance of any doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants or compounds, whether in polymeric form or otherwise, unless stated to the contrary. Conversely, the term "consisting essentially of excludes any other components, steps or procedures (except those that are not essential to operability) from the scope of any subsequent statements. The term "consisting of" excludes any components, steps or procedures that are not specifically described or listed. Unless otherwise stated, the term "or" refers to the listed members individually and in any combination.

[0035] An "ethylene-based polymer" is a polymer that contains more than 50 weight percent (wt%) polymerized ethylene monomer (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" are used interchangeably. Ethylene-based polymers may include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). 12 α-olefin or C4-C8 α-olefin) and / or ethylene copolymerized with unsaturated ester.

[0036] As used herein, the term "ethylene monomer" or "ethylene" refers to a chemical unit having two carbon atoms with a double bond therebetween, and each carbon bonded to two hydrogen atoms, wherein the chemical unit is polymerized with other such chemical units to form an ethylene-based polymer composition.

[0037] A "heteroatom" is an atom other than carbon or hydrogen. A heteroatom can be a non-carbon atom from Group IV, Group V, Group VI, and Group VII of the periodic table. Non-limiting examples of heteroatoms include: F, N, O, P, B, S, and Si.

[0038] A "hydrocarbon" is a compound containing only hydrogen and carbon atoms. A "hydrocarbon group" (or "hydrocarbon group") is a hydrocarbon having a valence (usually a single valence). A hydrocarbon may have a straight chain structure, a cyclic structure, or a branched structure.

[0039] "Linear low density polyethylene" (or "LLDPE") is a linear ethylene / α-olefin copolymer containing a heterogeneous distribution of short chain branches, the copolymer comprising units derived from ethylene and units derived from at least one C3-C 10 Units of at least one C4-C8 alpha-olefin comonomer or at least one C6-C8 alpha-olefin comonomer. LLDPE is characterized by minimal long chain branching (if any) compared to conventional LDPE. LLDPE has a density of 0.910 g / cc, or 0.915 g / cc, or 0.920 g / cc, or 0.925 g / cc to 0.930 g / cc, or 0.935 g / cc, or 0.940 g / cc. Non-limiting examples of LLDPE include TUFLIN, each available from The Dow Chemical Company, TM Linear low density polyethylene resin and DOWLEX TM Polyethylene resin; and MARLEX TM Polyethylene (available from Chevron Phillips).

[0040] "Low density polyethylene" (or "LDPE") consists of ethylene homopolymer or ethylene copolymer with acrylate, vinyl acetate and / or vinyl silane as comonomers, having a density of 0.915 g / cc to 0.940 g / cc and containing long chain branching and broad MWD. ​​LDPE is typically produced by high pressure free radical polymerization (tubular reactor or autoclave with free radical initiator). Non-limiting examples of LDPE include MarFlex TM (Chevron Phillips Company), LUPOLEN TM (LyondellBasell) and LDPE products from Borealis, Ineos, ExxonMobil, etc.

[0041] "Medium density polyethylene" (or "MDPE") is an ethylene homopolymer or a copolymer comprising at least one C3-C 10An ethylene / α-olefin copolymer of an α-olefin or a C3-C4 α-olefin having a density of 0.926 g / cc to 0.940 g / cc.

[0042] An "olefin" is an unsaturated aliphatic hydrocarbon having a carbon-carbon double bond.

[0043] "Olefin-based polymers" (interchangeably referred to as "polyolefins") are polymers that contain a majority weight % of polymerized olefin monomers (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers and propylene-based polymers.

[0044] As used herein, the term "polymer" or "polymeric material" refers to a compound prepared by polymerizing monomers, whether monomers of the same type or different types, which provide multiple and / or repeating "units" or "monomer units" constituting the polymer in a polymerized form. Therefore, the general term polymer covers the term homopolymer, which is usually used to refer to polymers prepared from only one type of monomer, and the term copolymer, which is usually used to refer to polymers prepared from at least two types of monomers. The general term also covers all forms of copolymers, such as random copolymers, block copolymers, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" represent copolymers prepared by polymerizing ethylene or propylene and one or more additional polymerizable α-olefin monomers, respectively, as described above. It should be noted that although polymers are generally referred to as "made of" one or more specified monomers, "based on" a specified monomer or monomer type, "containing" a specified monomer content, etc., in this context, the term "monomer" should be understood to refer to the polymerized residue of the specified monomer rather than the unpolymerized substance. In general, polymers are referred to herein as "units" based on the polymerized form of the corresponding monomers.

[0045] A "propylene-based polymer" is a polymer that contains more than 50 weight percent polymerized propylene monomer (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). The terms "propylene-based polymer" and "polypropylene" are used interchangeably. Non-limiting examples of propylene-based polymers (polypropylenes) are polypropylenes having at least one C2 or C4-C 10 Propylene / α-olefin copolymers with α-olefin comonomers.

[0046] "Sheath" refers to the cable covering and includes insulating coverings or layers, protective jackets, and the like.

[0047] As used herein, "silane" is a compound having one or more Si-C bonds.

[0048] As used herein, "siloxane" is a formulation having one or more Si-O-Si bonds.

[0049] Test Method

[0050] Burning test .

[0051] The vertical burning test was performed on 2 mm thick specimens in a UL94 (Underwriter's Laboratories 94) chamber according to the UL94 specification provided below.

[0052] • Before the test begins, place the plastic samples vertically in the combustion chamber. The dimensions of each sample are 127 mm x 12.7 mm, with a thickness of 2 mm.

[0053] After the sample is mounted, place a carefully controlled flame under the sample for 10 seconds and then remove it. When the flame is no longer in contact with the sample, observe and record any residual flaming combustion of the plastic sample.

[0054] • When the plastic sample finally self-extinguishes, immediately reapply a controlled flame for an additional 10 seconds and then remove. Again, record the flaming combustion of the sample (in the absence of flame exposure).

[0055] - Position a piece of dry surgical cotton 12 inches below the burning sample. If any droplets fall onto the cotton and cause it to ignite, this detail is also recorded.

[0056] Density is measured according to ASTM D792, Method B. Results are reported in grams per cubic centimeter (g / cc).

[0057] Melt index .

[0058] As used herein, the term "melt index" or "MI" refers to a measure of the ease with which a thermoplastic polymer flows in the molten state. Melt index or I2 is measured according to ASTM D 1238, Condition 190°C / 2.16 kg, and is reported in grams eluted per 10 minutes (g / 10 min). I10 is measured according to ASTM D 1238, Condition 190°C / 10 kg, and is reported in grams eluted per 10 minutes (g / 10 min).

[0059] Nuclear Magnetic Resonance (NMR)

[0060] 1H-NMR was used to characterize the molecular structure using a Bruker NMR spectrometer (400 MHz). 20 mg of the sample was dissolved in 0.5 ml of CDCl3 for 1 H-NMR test.

[0061] 13 C-NMR was used to characterize the molecular structure using a Bruker NMR spectrometer (100 MHz). 20 mg of sample was dissolved in 0.5 ml CDCl3 for 13 C-NMR test.

[0062] Thermogravimetric analysis (TGA) was performed using a flow cytometer from TA INSTRUMENTS TM Thermogravimetric analysis was performed using a Q5000 thermogravimetric analyzer. Thermogravimetric analysis was performed by placing a material sample in a thermogravimetric analyzer on a platinum plate at a flow rate of 25 cm 3 / min nitrogen, and after equilibration at 40°C, the temperature was raised from 40°C to 650°C at a rate of 20°C / min, and the air was exchanged, and heated from 650°C to 800°C at a rate of 20°C / min. The mass percentage retained at 650°C is a measure of the residue obtained in the form of char, and this value is recorded. That is, this TGA method characterizes the char formation of the flame retardant. A higher residue indicates better char formation. DETAILED DESCRIPTION

[0063] 1.Tetrabromophthalic anhydride diamine siloxane

[0064] In one embodiment, the present disclosure relates to a tetrabromophthalic anhydride diamine siloxane (TDS). The TDS has the structure of the following formula (1):

[0065] Formula (1)

[0066]

[0067] wherein n is an integer from 1 to 40, or from 2 to 30, or from 3 to 20, or from 4 to 15; and

[0068] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.

[0069] In one embodiment, the preparation of TDS is carried out by reacting tetrabromophthalic anhydride (TBPA) with an alkylaminoalkyl disiloxane such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane (BAPTMDS), for example, in a solvent such as tetrahydrofuran under reflux for two to six hours or four hours. The disiloxane moiety in the alkylaminoalkyl disiloxane promotes the formation of TDS, which is linear in structure. The reaction involves imidization between the amine groups of the alkylaminoalkyl disiloxane and the anhydride in the TBPA, and connects two TBPA units through the alkylaminoalkyl disiloxane.

[0070] In one embodiment, the TDS having the structure of formula (1) has a molecular weight of 1,000 g / mol to 5,000 g / mol, or 1,500 g / mol to 4,000 g / mol, or 2,000 g / mol to 3,000 g / mol. In another embodiment, n=20, and the TDS having the structure of formula (1) has a molecular weight of 2640 g / mol.

[0071] In one embodiment, the TDS has the structure of formula (2)

[0072] Formula (2)

[0073]

[0074] 2. Polymer composition

[0075] The present disclosure provides a polymer composition. The polymer composition comprises a TDS having a structure of formula (1). In one embodiment, the polymer composition comprises a polyolefin (e.g., a silane-functionalized polyolefin) and a TDS having a structure of formula (1):

[0076] Formula (1)

[0077]

[0078] wherein n is an integer from 1 to 40, or from 2 to 30, or from 3 to 20, or from 4 to 15; and

[0079] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.

[0080] In one embodiment, the polymer composition comprises a silane functionalized polyolefin.As used herein, a "silane functionalized polyolefin" is a polymer containing a silane and greater than 50 weight percent or a majority amount of polymerized ethylene based on the total weight of the silane functionalized polyolefin.

[0081] In one embodiment, the silane-functionalized polyolefin is a silane-functionalized ethylene-based polymer. A "silane-functionalized ethylene-based polymer" is a polymer containing silane and greater than 50 weight percent or a majority amount of polymerized ethylene based on the total weight of the polymer. Non-limiting examples of suitable silane-functionalized polyolefins include ethylene / silane copolymers, silane-grafted polyethylene (Si-g-PE), and combinations thereof.

[0082] "Ethylene / silane copolymers" are formed by copolymerizing ethylene with hydrolyzable silane monomers (e.g., vinyl-alkoxysilane monomers). In one embodiment, ethylene / silane copolymers are prepared by copolymerizing ethylene, hydrolyzable silane monomers, and optionally unsaturated esters. The preparation of ethylene / silane copolymers is described, for example, in USP 3,225,018 and USP 4,574,133, each of which is incorporated herein by reference.

[0083] "Silane grafted polyolefins" (or "Si-g-PE") are formed by grafting hydrolyzable silane monomers (such as vinyl alkoxy silane monomers) onto the backbone of a base polyethylene. In one embodiment, the grafting occurs in the presence of a free radical generator (such as a peroxide). The hydrolyzable silane monomers can be (i) incorporated into or compounded into a composition (also known as SIOPLAS) for making a final article (such as a coated conductor) or (ii) in a prepolymer (also known as a prepolymer) (e.g., a prepolymer) containing a hydrolyzable silane monomer. TM method), or (ii) with extrusion of the composition to form a final article (also known as MONOSIL TM The method comprises the steps of: forming Si-g-PE in situ during melt blending and extrusion and grafting the Si-g-PE to the backbone of the base polyethylene. In one embodiment, the Si-g-PE is formed before the Si-g-PE is compounded with the inorganic hollow microspheres and other optional components. In another embodiment, the Si-g-PE is formed in situ by compounding the polyethylene, the hydrolyzable silane monomer and the peroxide initiator, and the inorganic hollow microspheres and other optional components.

[0084] The base polyethylene of Si-g-PE can be any ethylene-based polymer disclosed herein. Non-limiting examples of suitable ethylene-based polymers include ethylene homopolymers and ethylene-based interpolymers containing one or more polymerizable comonomers (such as unsaturated esters and / or α-olefins). In one embodiment, the ethylene-based polymer is selected from low density polyethylene (LDPE), high density polyethylene (HDPE) and combinations thereof.

[0085] A "hydrolyzable silane monomer" is a silane-containing monomer that will effectively copolymerize with an α-olefin (e.g., ethylene) to form an α-olefin / silane copolymer (e.g., ethylene / silane copolymer), or graft to an α-olefin polymer (i.e., polyolefin) to form a Si-g-polyolefin, thereby achieving subsequent crosslinking of the silane-functionalized polyolefin. A representative but non-limiting example of a hydrolyzable silane monomer has structure (I):

[0086]

[0087] Where R 1 is a hydrogen atom or a methyl group; x is 0 or 1; n is an integer from 1 to 4, or 6, or 8, or 10 or 12; and each R 2 are independently hydrolyzable organic groups, such as alkoxy groups having 1 to 12 carbon atoms (e.g., methoxy, ethoxy, butoxy), aryloxy groups (e.g., phenoxy), aralkyloxy groups (e.g., benzyloxy), aliphatic acyloxy groups having 1 to 12 carbon atoms (e.g., formyloxy, acetoxy, propionyloxy), amino or substituted amino groups (e.g., alkylamino, arylamino), or lower alkyl groups having 1 to 6 carbon atoms, provided that the three R 2 No more than one of the groups is an alkyl group. The hydrolyzable silane monomer can be copolymerized (such as a high pressure process) with an alpha-olefin (such as ethylene) in a reactor to form an alpha-olefin / silane copolymer. In the example where the alpha-olefin is ethylene, this copolymer is referred to herein as an ethylene / silane copolymer. The hydrolyzable silane monomer can also be grafted to a polyolefin (such as polyethylene) using an organic peroxide such as 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane to form Si-g-PO or in-situ Si-g-PO. In-situ Si-g-PO is formed by a process such as the MONOSIL process, in which during extrusion of the composition of the present invention to form a coated conductor, the hydrolyzable silane monomer is grafted to the backbone of the polyolefin, as described, for example, in USP 4,574,133.

[0088] The hydrolyzable silane monomer may include a silane monomer comprising an ethylenically unsaturated hydrocarbon group (such as a vinyl, allyl, isopropenyl, butenyl, cyclohexenyl or γ-(meth)acryloxyallyl group) and a hydrolyzable group (such as, for example, a hydrocarbonoxy, hydrocarbon acyloxy or hydrocarbon amino group). The hydrolyzable group may include a methoxy, ethoxy, formyloxy, acetoxy, propionyloxy and alkyl or arylamino group. In a specific example, the hydrolyzable silane monomer is an unsaturated alkoxysilane that can be grafted onto a polyolefin or copolymerized with an α-olefin (such as ethylene) in a reactor. Examples of hydrolyzable silane monomers include vinyltrimethoxysilane (VTMS), vinyltriethoxysilane (VTES), vinyltriacetoxysilane and γ-(meth)acryloxypropyltrimethoxysilane. In the context of structure (I), for VTMS: x=0; R 1 = hydrogen; and R 2 = methoxy; for VTES: x = 0; R 1 = hydrogen; and R 2 =ethoxy; and for vinyltriacetoxysilane: x=0; R 1 =H; and R 2 =Acetoxy.

[0089] Examples of suitable ethylene / silane copolymers can be found in SI-LINK, VIZIONE ... TM DFDA-5451NT and SI-LINK TM AC DFDB-5451NT is commercially available. Examples of suitable Si-g-PO include PEXIDAN TM A-3001 is commercially available from SACO AEI Polymers (Sheboygan, WI) and as SYNCURE TM S1054A was commercially available from PolyOne (Avon Lake, OH).

[0090] In one embodiment, the silane-functionalized ethylene-based polymer contains from 0.1 wt%, or 0.3 wt%, or 0.5 wt%, or 0.8 wt%, or 1.0 wt%, or 1.2 wt%, or 1.5 wt%, or 1.6 wt% to 1.8 wt%, or 2.0 wt%, or 2.3 wt%, or 2.5 wt%, or 3.0 wt%, or 3.5 wt%, or 4.0 wt%, or 4.5 wt%, or 5.0 wt% silane, based on the total weight of the silane-functionalized ethylene-based polymer.

[0091] In one embodiment, the silane-functionalized ethylene-based polymer contains (i) 50 wt%, or 55 wt%, or 60 wt%, or 65 wt%, or 70 wt%, or 80 wt%, or 90 wt%, or from 95 wt% to 97 wt%, or 98 wt%, or 99 wt%, or less than 100 wt% ethylene and (ii) 0.1 wt%, or 0.3 wt%, or 0.5 wt%, or 0.8 wt%, or 1.0 wt%, or 1.2 wt%, or 1.5 wt%, or from 1.6 wt% to 1.8 wt%, or 2.0 wt%, or 2.3 wt%, or 2.5 wt%, or 3.0 wt%, or 3.5 wt%, or 4.0 wt%, or 4.5 wt%, or 5.0 wt% silane, based on the total weight of the silane-functionalized polyethylene.

[0092] In one embodiment, the silane functionalized ethylene-based polymer has a density of 0.850 g / cc, or 0.860 g / cc, or 0.875 g / cc, or 0.890 g / cc, or 0.900 g / cc, or 0.910 g / cc, or 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, or 0.930 g / cc, or 0.940 g / cc, or 0.950 g / cc or 0.960 g / cc, or 0.965 g / cc. In another embodiment, the silane functionalized ethylene-based polymer has a density of 0.850 g / cc to 0.965 g / cc, or 0.900 g / cc to 0.950 g / cc, or 0.920 g / cc to 0.925 g / cc.

[0093] In one embodiment, the silane-functionalized ethylene-based polymer has a melt index (MI) of 0.1 g / 10 min, or 0.5 g / 10 min, or 1.0 g / 10 min, or 1.5 g / 10 min to 6 g / 10 min, or 10 g / 10 min, or 15 g / 10 min, or 20 g / 10 min, or 30 g / 10 min, or 40 g / 10 min, or 50 g / 10 min. In another embodiment, the functionalized ethylene-based polymer has a melt index (MI) of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 10 g / 10 min.

[0094] In one embodiment, the silane functionalized ethylene-based polymer is an ethylene / silane copolymer. The ethylene / silane copolymer contains ethylene and a hydrolyzable silane monomer as the only monomer units. In another embodiment, the ethylene / silane copolymer optionally includes C3, or C4 to C6, or C8, or C 10 , or C 12 , or C 16 , or C 18, or C 20 α-olefins; unsaturated esters; and combinations thereof. In one embodiment, the ethylene / silane copolymer is an ethylene / unsaturated ester / silane reactor copolymer. Non-limiting examples of suitable ethylene / silane copolymers include SI-LINK, each available from The Dow Chemical Company. TM DFDA-5451NT and SI-LINK TM AC DFDB-5451NT.

[0095] An ethylene / silane copolymer may comprise two or more embodiments disclosed herein.

[0096] In one embodiment, the silane-functionalized ethylene-based polymer is Si-g-PE.

[0097] The base ethylene-based polymer for Si-g-PE comprises 50 wt%, or 55 wt%, or 60 wt%, or 65 wt%, or 70 wt%, or 80 wt%, or 90 wt%, or 95 wt% to 97 wt%, or 98 wt%, or 99 wt%, or 100 wt% ethylene, based on the total weight of the base ethylene-based polymer.

[0098] In one embodiment, the density of the base ethylene-based polymer for Si-g-PE is 0.850 g / cc, or 0.860 g / cc, or 0.875 g / cc, or 0.890 g / cc, or 0.900 g / cc, or 0.910 g / cc, or 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, or 0.930 g / cc, or 0.940 g / cc, or 0.950 g / cc or 0.960 g / cc, or 0.965 g / cc. In another embodiment, the density of the base ethylene-based polymer for Si-g-PE is 0.850 g / cc to 0.965 g / cc, or 0.900 g / cc to 0.950 g / cc, or 0.920 g / cc to 0.925 g / cc.

[0099] In one embodiment, the base ethylene-based polymer for Si-g-PE has a melt index (MI) of 0.1 g / 10 min, or 0.5 g / 10 min, or 1.0 g / 10 min, or 1.5 g / 10 min to 6 g / 10 min, or 10 g / 10 min, or 15 g / 10 min, or 20 g / 10 min, or 30 g / 10 min, or 40 g / 10 min, or 50 g / 10 min. In another embodiment, the base ethylene-based polymer for Si-g-PE has a melt index (MI) of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 10 g / 10 min.

[0100] In one embodiment, the base ethylene-based polymer for Si-g PE is an ethylene / α-olefin copolymer. The α-olefin contains 3, or 4 to 6, or 8, or 10, or 12, or 16, or 18, or 20 carbon atoms. Non-limiting examples of suitable α-olefins include propylene, butene, hexene and octene. In one embodiment, the ethylene-based copolymer is an ethylene / octene copolymer. When the ethylene-based copolymer is an ethylene / α-olefin copolymer, the Si-g-PE is a silane-grafted ethylene / α-olefin copolymer. Non-limiting examples of suitable ethylene / α-olefin copolymers used as the base ethylene-based polymer for Si-g-PE include ENGAGE TM and INFUSE TM Resin.

[0101] In one embodiment, the base ethylene-based polymer for Si-g-PE is a low density polyethylene (LDPE). LDPE has a density of 0.915 g / cc to 0.940 g / cc and contains long chain branching and broad MWD. ​​In one embodiment, the density of LDPE is 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, or 0.930 g / cc, or 0.940 g / cc.

[0102] In one embodiment, Si-g-PE is a silane-grafted ethylene / C4-C8 α-olefin copolymer. The silane-grafted ethylene / C4-C8 α-olefin copolymer consists of a hydrolyzable silane monomer, ethylene, and a C4-C8 α-olefin comonomer. In other words, the silane-grafted ethylene / C4-C8 α-olefin copolymer contains a hydrolyzable silane monomer, ethylene, and a C4-C8 α-olefin comonomer as the only monomer units.

[0103] In one embodiment, the Si-g-PE is a silane-grafted LDPE ("Si-g-LDPE"). The Si-g-LDPE has one, some or all of the following properties: (i) a density of 0.915 g / cc to 0.940 g / cc or 0.920 g / cc to 0.930 g / cc; and / or (ii) a melt index of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 10 g / 10 min; and / or (iii) a silane content of 0.1 wt% to 5 wt%, or 0.5 wt% to 3.0 wt%, based on the total weight of the Si-g-LDPE. In another embodiment, the Si-g-LDPE consists of a hydrolyzable silane monomer, ethylene, and a C4-C8 α-olefin comonomer.

[0104] The Si-g-PE may comprise two or more embodiments disclosed herein.

[0105] Blends of silane-functionalized olefin-based polymers may also be used, and the silane-functionalized ethylene-based polymer may be diluted with one or more other polyolefins to the extent that the polyolefins (i) are miscible or compatible with each other, and (ii) the silane-functionalized ethylene-based polymer comprises from 50 wt%, or 55 wt%, or 60 wt%, or 65 wt%, or 70 wt%, or 75 wt%, or 80 wt%, or 85 wt%, or 90 wt%, or 95 wt%, or 98 wt%, or 99 wt% to less than 100 wt% of the blend (based on the combined weight of the polyolefins including the silane-functionalized ethylene-based polymer).

[0106] The silane-functionalized ethylene-based polymer may include two or more embodiments disclosed herein.

[0107] In addition to the silane-functionalized polyolefin, the polymer composition also includes a TDS having a structure of formula (1) or a TDS having a structure of formula (2). TDS is a flame retardant of the polymer composition. The polymer composition includes 50 wt % to 95 wt % of a silane-functionalized polyolefin and 50 wt % to 5 wt % of a TDS, or 60 wt % to 90 wt % of a silane-functionalized polyolefin and 40 wt % to 10 wt % of a TDS, and the silane-functionalized polyolefin and the TDS account for 100 wt % of the polymer composition.

[0108] In one embodiment, the polymer composition comprises a silane-functionalized polyolefin (which is an ethylene / silane copolymer), a TDS having a structure of formula (1), a flame retardant synergist, and an optional second polyolefin. As used herein, a "flame retardant synergist" is a compound that improves the flame retardant properties of the TDS. Non-limiting examples of suitable flame retardant synergists include antimony trioxide (Sb2O3), zinc borate, zinc carbonate, zinc carbonate hydroxide, hydrated zinc borate, zinc phosphate, zinc stannate, zinc hydroxystannate, zinc sulfide, zinc oxide, and combinations thereof.

[0109] The second polyolefin (when present) can be an ethylene-based polymer or a propylene-based polymer. In one embodiment, the second polyolefin is an ethylene-based polymer, and the ethylene-based polymer is an ethylene / C3-C8 alpha-olefin copolymer or an ethylene / C4-C8 alpha-olefin copolymer. Non-limiting examples of suitable alpha-olefins include propylene, butene, hexene and octene. In one embodiment, the ethylene-based copolymer is an ethylene / octene copolymer. Non-limiting examples of suitable ethylene / octene copolymers include DOWLEX® available from The Dow Chemical Company. TM RESIN AND / OR ENGAGE TMResin.

[0110] 3. Additives

[0111] The polymer composition may include one or more optional additives. Non-limiting examples of suitable additives include antioxidants, colorants, corrosion inhibitors, lubricants, moisture curing catalysts, ultraviolet (UV) absorbers or stabilizers, anti-caking agents, coupling agents, compatibilizers, plasticizers, fillers, processing aids, and combinations thereof.

[0112] In one embodiment, the polymer composition comprises an antioxidant. Non-limiting examples of suitable antioxidants include phenolic antioxidants, sulfur-based antioxidants, phosphate-based antioxidants, and hydrazine-based metal passivators. Suitable phenolic antioxidants include high molecular weight hindered phenols, methyl-substituted phenols, phenols with primary or secondary carbonyl substituents, and multifunctional phenols such as sulfur-containing and phosphorus-containing phenols. Representative hindered phenols include 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; pentaerythritol tetrakis-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate; n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; 4,4'-methylenebis(2,6-tert-butyl-phenol); 4,4'-thiobis(6-tert-butyl-o-cresol) 2,6-di-tert-butylphenol; 6-(4-hydroxyphenoxy)-2,4-bis(n-octyl-thio)-l,3,5-triazine; 3,5-di-tert-butyl-4-hydroxybenzoic acid (di-n-octylthio) ethyl ester; and hexa[3-(3,5-di-tert-butyl-4-hydroxy-phenyl)-propionate] sorbitol ester. In one embodiment, the polymer composition includes Irganox TM 1010 pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate commercially available from BASF. A non-limiting example of a suitable methyl-substituted phenol is isobutylidene bis(4,6-dimethylphenol). A non-limiting example of a suitable hydrazine-based metal deactivator is oxalyl bis(benzylidene hydrazide). In one embodiment, the polymer composition contains 0 wt%, or 0.001 wt%, or 0.01 wt%, or 0.02 wt%, or 0.05 wt%, or 0.1 wt%, or 0.2 wt%, or 0.3 wt%, or 0.4 wt% to 0.5 wt%, or 0.6 wt%, or 0.7 wt%, or 0.8 wt%, or 1.0 wt%, or 2.0 wt%, or 2.5 wt%, or 3.0 wt% of an antioxidant based on the total weight of the polymer composition.

[0113] In one embodiment, the polymer composition comprises a moisture curing catalyst, such as a Lewis acid and a Bronsted acid and / or a Lewis base and a Bronsted base. As used herein, a "moisture curing catalyst" is a compound that promotes the cross-linking of silane-functionalized polyolefins by hydrolysis and condensation reactions. Lewis acids are chemical species that can accept electron pairs from Lewis bases. Lewis bases are chemical substances that can accept electron pairs from Lewis bases. Non-limiting examples of suitable Lewis acids include carboxylates such as dibutyltin dilaurate (DBTDL), dimethylhydroxytin oleate, dioctyltin maleate, di-n-butyltin maleate, dibutyltin diacetate, dibutyltin dioctoate, stannous acetate, stannous octoate, and various other organometallic compounds such as lead naphthenate, zinc octoate, and cobalt naphthenate. Non-limiting examples of suitable Lewis bases include primary amines, secondary amines, and tertiary amines. Non-limiting examples of suitable Bronsted acids are methanesulfonic acid, benzenesulfonic acid, dodecylbenzenesulfonic acid, naphthalenesulfonic acid, or alkylnaphthalenesulfonic acid. Moisture curing catalyst can include blocked sulfonic acid. Blocked sulfonic acid can be as defined in US 2016 / 0251535A1, and can be a compound that generates sulfonic acid in situ when heated, optionally in the presence of moisture or alcohol. Examples of blocked sulfonic acid include amine-sulfonate and alkyl sulfonate. Blocked sulfonic acid can be composed of carbon atoms, hydrogen atoms, a sulfur atom and three oxygen atoms and optional nitrogen atoms. These catalysts are generally used in moisture curing applications. Based on the gross weight of the composition, the polymer composition includes 0 wt %, or 0.001 wt %, or 0.005 wt %, or 0.01 wt %, or 0.02 wt %, or 0.03 wt % to 0.05 wt %, or 0.1 wt %, or 0.2 wt %, or 0.5 wt %, or 1.0 wt %, or 3.0 wt %, or 5.0 wt %, or 10 wt %, or 20 wt % of moisture curing catalyst. Moisture cure catalysts are typically added to the article manufacturing extruder (e.g., during cable manufacturing) so that they are present during the final melt extrusion process. Thus, the silane-functionalized polyolefin may undergo some crosslinking before it leaves the extruder, wherein the crosslinking is completed after it leaves the extruder (typically after exposure to moisture (e.g., sauna, hot or cold bath) and / or humidity present in the environment in which it is stored, transported, or used.

[0114] The moisture curing catalyst may be included in a catalyst masterbatch blend, wherein the catalyst masterbatch is included in the polymer composition. Non-limiting examples of suitable catalyst masterbatches include those sold by The Dow Chemical Company under the trade name SI-LINK TM Catalyst masterbatches for sale, including SI-LINK TM DFDA-5481Natural and SI-LINK TMAC DFDA-5488NT. In one embodiment, the polymer composition contains 0 wt%, or 0.001 wt%, or 0.01 wt%, or 0.5 wt%, or 1.0 wt%, or 2.0 wt%, or 3.0 wt%, or 4.0 wt% to 5.0 wt%, or 6.0 wt%, or 7.0 wt%, or 8.0 wt%, or 9.0 wt%, or 10.0 wt%, or 15.0 wt%, or 20.0 wt% of a moisture cure catalyst based on the total weight of the polymer composition.

[0115] In one embodiment, the polymer composition includes an ultraviolet (UV) absorber or stabilizer. Non-limiting examples of suitable UV stabilizers are hindered amine light stabilizers (HALS). Non-limiting examples of suitable HALS are 1,3,5-triazine-2,4,6-triamine, N,N-1,2-ethanediylbis-N-3-4,6-dibutyl(1,2,2,6,6-pentamethyl-4-piperidinyl)amino-1,3,5-triazine-2-ylaminopropyl-N,N-dibutyl-N,N-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-1,5,8,12-tetrakis[4,6-bis(n-butyl-n-1,2,2,6,6-pentamethyl-4-piperidinylamino)-1,3,5-triazine-2-yl]-1,5,8,12-tetraazadodecane, which can be SABO TM STAB UV-119 is commercially available from SABO SpA of Levate, Italy. In one embodiment, the composition contains 0 wt%, or 0.001 wt%, or 0.002 wt%, or 0.005 wt%, or 0.006 wt% to 0.007 wt%, or 0.008 wt%, or 0.009 wt%, or 0.01 wt%, or 0.2 wt%, or 0.3 wt%, or 0.4 wt%, or 0.5 wt%, 1.0 wt%, or 2.0 wt%, or 2.5 wt%, or 3.0 wt% of a UV absorber or stabilizer, based on the total weight of the polymer composition.

[0116] In one embodiment, the polymer composition comprises a filler. Non-limiting examples of suitable fillers include carbon black, organoclay, aluminum hydroxide, magnesium hydroxide, calcium carbonate, hydromagnesite, magnesite, hydrotalcite, boehmite, magnesium carbonate, magnesium phosphate, calcium hydroxide, calcium sulfate, silicon dioxide, silicone rubber, talc, and combinations thereof. The filler may or may not have flame retardant properties. In one embodiment, the filler is coated with a material that will prevent or stop any tendency that the filler may otherwise have to interfere with the silane curing reaction. Stearic acid illustrates such a filler coating. In one embodiment, the polymer composition contains 0 wt%, or 0.01 wt%, or 0.02 wt%, or 0.05 wt%, or 0.07 wt%, or 0.1 wt%, or 0.2 wt%, or 0.3 wt%, or 0.4 wt% to 0.5 wt%, or 0.6 wt%, or 0.7 wt%, or 0.8 wt%, or 1.0 wt%, or 2.0 wt%, or 2.5 wt%, or 3.0 wt%, or 5.0 wt%, or 8.0 wt%, or 10.0 wt%, or 20 wt% filler, based on the total weight of the polymer composition.

[0117] In one embodiment, the polymer composition includes a processing aid. Non-limiting examples of suitable processing aids include oils, polydimethylsiloxanes, organic acids (such as stearic acid) and metal salts of organic acids (such as zinc stearate). In one embodiment, based on the gross weight of the polymer composition, the polymer composition contains 0 wt %, or 0.01 wt %, or 0.02 wt %, or 0.05 wt %, or 0.07 wt %, or 0.1 wt %, or 0.2 wt %, or 0.3 wt %, or 0.4 wt % to 0.5 wt %, or 0.6 wt %, or 0.7 wt %, or 0.8 wt %, or 1.0 wt %, or 2.0 wt %, or 2.5 wt %, or 3.0 wt %, or 5.0 wt %, or 10.0 wt % of processing aid.

[0118] In one embodiment, the polymer composition contains 0 wt%, or greater than 0 wt%, or 0.001 wt%, or 0.002 wt%, or 0.005 wt%, or 0.006 to 0.007 wt%, or 0.008 wt%, or 0.009 wt%, or 0.01 wt%, or 0.2 wt%, or 0.3 wt%, or 0.4 wt%, or 0.5 wt%, 1.0 wt%, or 2.0 wt%, or 2.5 wt%, or 3.0 wt%, or 4.0 wt%, or 5.0 to 6.0 wt%, or 7.0 wt%, or 8.0 wt%, or 9.0 wt%, or 10.0 wt%, or 15.0 wt%, or 20.0 wt%, or 30 wt%, or 40 wt%, or 50 wt% of the additive, based on the total weight of the polymer composition.

[0119] In one embodiment, the polymer composition comprises

[0120] (A) 35 to 55 wt % or 40 to 50 wt % of an ethylene / silane copolymer;

[0121] (B) 15 to 35 wt % or 20 to 30 wt % of a flame retardant, wherein the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1) or a structure of formula (2);

[0122] (C) 10 to 20 wt % or 12 to 18 wt % of a first flame retardant synergist, the first flame retardant synergist being antimony trioxide;

[0123] (D) 1 to 10 wt % or 2 to 7 wt % of a second flame retardant synergist,

[0124] The second flame retardant synergist is zinc oxide;

[0125] (E) from greater than 0 wt % to 7 wt % or from 2 wt % to 6 wt % of a moisture cure catalyst;

[0126] (F) 0 wt%, or from greater than 0 wt%, to 7 wt%, or from 2 wt% to 6 wt%, of a second polyolefin that is an ethylene-based polymer; and

[0127] (G) 0 wt % or more to 0.5 wt % or 0.05 wt % to 0.4 wt % antioxidant;

[0128] The aggregate of components (A) to (G) accounts for 100% by weight of the polymer composition.

[0129] In one embodiment, the polymer composition comprises

[0130] (A) 35 to 55 wt % or 40 to 50 wt % of an ethylene / silane copolymer;

[0131] (B) 15 to 35 wt % or 20 to 30 wt % of a flame retardant, wherein the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1) or a structure of formula (2);

[0132] (C) 10 to 20 wt % or 12 to 18 wt % of a first flame retardant synergist, the first flame retardant synergist being antimony trioxide;

[0133] (D) 1 to 10 wt % or 2 to 7 wt % of a second flame retardant synergist,

[0134] The second flame retardant synergist is zinc oxide;

[0135] (E) 0 wt %, or from greater than 0 wt % to 7 wt %, or from 2 wt % to 6 wt % of a moisture cure catalyst;

[0136] (F) 0 wt%, or from greater than 0 wt%, to 7 wt%, or from 2 wt% to 6 wt%, of a second polyolefin that is an ethylene-based polymer;

[0137] (G) 0 wt % or more to 0.5 wt % or 0.05 wt % to 0.4 wt % antioxidant;

[0138] The aggregate of components (A) to (G) accounts for 100% by weight of the polymer composition.

[0139] 4. Cable

[0140] The present disclosure provides a cable. In one embodiment, the cable comprises (i) a conductor and (ii) a coating on the conductor. The coating comprises a polymer composition consisting of (i) a silane-functionalized polyolefin and (ii) a tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1) or having a structure of formula (2).

[0141] As used herein, a "conductor" is one or more wires or fibers used to conduct heat, light, and / or electricity. The conductor can be a single wire / fiber or multiple wires / fibers and can be in stranded form or tubular form. Non-limiting examples of suitable conductors include metals such as silver, gold, copper, carbon, and aluminum. The conductor can also be an optical fiber made of glass or plastic.

[0142] As used herein, a "cable" is at least one wire or optical fiber within a sheath, such as an insulating sheath or a protective outer sheath. Typically, a cable is two or more wires or two or more optical fibers that are usually bundled together in a common insulating sheath and / or protective sheath. The individual wires or fibers in the sheath may be bare, covered or insulated. A combination cable may contain both wires and optical fibers. The cable may be designed for low voltage, medium voltage and / or high voltage applications. An AC cable may be prepared according to the present disclosure, which may be a low voltage, medium voltage, high voltage or ultra-high voltage cable. Further, a DC cable may be prepared according to the present disclosure, which may include a high voltage or ultra-high voltage cable. An insulated electric conductor typically includes a conductive core covered by an insulating layer. The conductive core may be solid or braided (e.g., a bundle of wires). Some insulated electric conductors may also contain one or more additional elements, such as one (or more) semiconductor layers and / or protective covers (e.g., coiled wires, tapes or sheaths). Examples are coated metallic conductors and power cables, including those used for low voltage ("LV", >0 to <5 kilovolt (kV) power distribution / transmission applications), medium voltage ("MV", 5kV to <69kV), high voltage ("HV", 69kV to 230kV), and extra high voltage ("EHV", >230kV). Power cable evaluations may use AEIC / ICEA standards and / or IEC test methods.

[0143] The cable comprises a conductor and a coating on the conductor. The coating comprises a polymer composition composed of a silane-functionalized polyolefin and a flame retardant (as previously disclosed herein), wherein the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having a structure of formula (1):

[0144] Formula (1)

[0145]

[0146] wherein n is an integer from 1 to 40, or from 2 to 30, or from 3 to 20, or from 4 to 15; and

[0147] Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.

[0148] In one embodiment, the TDS has the structure of formula (2).

[0149] The polymer composition in the coating may comprise components (A)-(G) as previously disclosed herein.

[0150] In one embodiment, the cable comprises a coating of a polymer composition, and the coating is a cross-linked insulation layer, which surrounds the conductor. In a further embodiment, the cross-linked insulation layer directly contacts the conductor. The term "direct contact" refers to a layer configuration in which the cross-linked insulation layer is positioned adjacent to the conductor and there is no intermediate layer or intermediate structure between the conductor and the cross-linked insulation layer. Alternatively, the cross-linked insulation layer directly contacts the conductor.

[0151] By way of example and not limitation, some embodiments of the present disclosure will now be described in detail in the following examples.

[0152] Example

[0153] The materials used in the comparative samples (CS) and the inventive examples (IE) are provided in Table 1 below.

[0154] Table 1

[0155]

[0156]

[0157] 1. Synthesis of Tetrabromophthalic Anhydride Siloxane (TDS)

[0158] (30mL) BAPTMDS (496mg, 2.0mmol) was added to a solution of TBPA (1.94g, 4.2mmol) in tetrahydrofuran (THF) solvent to form a reaction mixture. The reaction mixture was then refluxed for 4 hours (h). Afterwards, the solvent (THF) was removed by a rotary evaporator, and the residue was dissolved in chloroform (CHCl3) and washed five times with warm water (60°C). After removing the chloroform, the off-white solid was dried overnight at 80°C in an oven. The yield of TDS having a structure of formula (2) was 94%. 1 HNMR (400MHz, CDCl3, ppm): δ3.67(t,J=7.5Hz,2H), 1.73–1.65(m,2H), 0.54(t,J=7.9Hz,2H), 0.05(s,2H). 13 C NMR (100MHz, CDCl3, ppm): δ163.9,137.4,130.8,121.2,41.9,22.3,15.4,0.3. FT-IR(KBr,cm -1 ):2968,2875,1714,1401,1344,1259,669.

[0159] The reaction pathway for synthesizing TDS having the structure of formula (2) is shown in the following reaction scheme (1).

[0160] Reaction scheme (1)

[0161]

[0162] Flame retardant TGA analysis

[0163] Table 2

[0164] Flame retardants Residue after testing Saytex BT-93W 0% Saytex HP-7010 0% TDS formula (2) 5%

[0165] As shown in Table 2, Saytex BT-93 and Saytex HP-7010 did not form char, while the TDS of the structure having the formula (2) reached 5% of the residue.

[0166] 2. Preparation of polymer composition

[0167] The ethylene / silane copolymer (PE1) and the second polyolefin (Dowlex 2047, where present) were fed into a Brabender mixer set at a temperature of 160°C and a rotor (roller rotor) speed of 15 rpm for 3 minutes (min) to melt the polymer (and the second polyolefin, where present). The antioxidant (AO), the first flame retardant synergist / second flame retardant synergist (ZnO, Sb2O3) and the flame retardant TDS having the structure of formula (2) were fed into the mixer, and then the rotor speed was increased to 50 rpm, and mixing was continued for 5 minutes. A moisture curing catalyst masterbatch (DFDA-5481) was then added, where mixing was continued for another 1 minute. The polymer composition was discharged from the Brabender mixer and formed into a 2 mm thick plate by compression molding at 125°C. The plate was cured in a 90°C water bath for 8 hours.

[0168] The vertical burning test results for the comparative sample (CS) and the inventive example (IE) are shown in Table 3 below.

[0169] Table 3: Polymer compositions and vertical burning test results

[0170]

[0171]

[0172] *Burnout - the flame will not go out until the sample is completely burned

[0173] & Flame time is the time between the removal of the fire and the self-extinguishing of the sample.

[0174] The Br content (in weight %) in Table 3 was calculated based on the following equation (A).

[0175] Equation (A)

[0176] Br content = 79.9 * the number of Br in the FR molecule * the percentage of FR in the composite material / Mw of FR

[0177] (a) According to the product manual, the Br content of Saytex BT-93W is 67.2 wt%

[0178] (b) According to the product manual, the Br content of Saytex HP 7010G is 68.5 wt %.

[0179] (c) Br content TDS formula (2) = 79.9*8 / 1131 = 56.5%

[0180] 79.9 is the Mw of Br

[0181] 8 is the number of Br in one molecule of TDS formula (2)

[0182] 1131 is the Mw of TDS formula (2)

[0183] (d) The Br content of each of CS1, CS2, IE1 and IE2 is calculated by the Wt.% of FR in each example*the Br content of FR

[0184] (i) CS1 = 25% * 67.2% = 16.8% by weight

[0185] (ii) CS2 = 24.4% * 68.5% = 16.7 wt%

[0186] (iii) IE1 = 29.4% * 57.2% = 16.8% by weight

[0187] (iv) IE2 = 29.4% * 56.5% = 16.6% by weight

[0188] For example, in Table 3, the value of "1 sec / 36 sec" of "Flame time after 1st agitation / Flame time after 2nd agitation" of CS1 Run #1 indicates that the flame automatically extinguishes within 1 second after the 1st agitation, and the flame automatically extinguishes within 36 seconds after the 2nd agitation.

[0189] Comparative sample 1 (CS1) with flame retardant Saytex BT-93W (a small molecule brominated flame retardant with a Mw of 951.5 g / mol) and CS2 with flame retardant Saytex HP 7010G (brominated polystyrene) were evaluated by inventive examples 1 (IE1) and IE2, each containing a flame retardant TDS of formula (2). As shown in Table 3, for CS1, the flame automatically extinguished immediately in the first agitation after the flame was removed. In the second agitation, CS1 automatically extinguished the flame in a short time. In CS1, Saytex BT-93W is known to have high PBT properties. In comparison, CS2 burned completely in the first agitation and did not automatically extinguish. It is known that Saytex HP 7010G has poor compatibility in the polyethylene matrix in CS2.

[0190] IE1 (flame retardant TDS of formula (2)) has a lower total Br content than CS2 (IE1 Br content 13.9 wt% vs. CS2 Br content 16.8 wt%). Even at a lower Br content than CS2, IE1 self-extinguished during the vertical flame test.

[0191] IE2 (flame retardant TDS with formula (2)) has a bromine content of 16.8 wt%, which is the same as the bromine content of CS1 and CS2. IE2, whose Br loading is at the same level as the Br loading of CS1 and CS2, has the same flame retardant properties as CS1.

[0192] It is particularly intended that the present disclosure is not limited to the embodiments and descriptions contained herein, but includes modifications of those embodiments including parts of the embodiments and combinations of elements of different embodiments as appear within the scope of the following claims.

Claims

1. A tetrabromophthalic anhydride diamine siloxane (TDS), wherein the TDS has a structure of formula (1): Formula (1) wherein n is an integer from 1 to 40; and Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of a hydrocarbon group; 2 . The TDS according to claim 1 , wherein the TDS having the structure of formula (1) has a molecular weight of 1,000 to 5,000 g / mol.

3. The TDS according to any one of claims 1 to 2, wherein the TDS has a structure of formula (2) Formula (2) 4. A polymer composition comprising: Flame retardant, the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having the structure of formula (1) Formula (1) wherein n is an integer from 1 to 40; and Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.

5. The polymer composition of claim 4, comprising a silane-functionalized polyolefin.

6. The polymer composition according to claim 5, comprising A silane-functionalized polyolefin, wherein the silane-functionalized polyolefin is an ethylene / silane copolymer; The TDS having the structure of formula (1); and Flame retardant synergist.

7. The polymer composition of claim 6, wherein the flame retardant synergist is selected from the group consisting of antimony trioxide, zinc oxide, and combinations thereof.

8. The polymer composition according to any one of claims 5 to 7, comprising a second polyolefin.

9. The polymer composition according to any one of claims 5 to 8, comprising a moisture curing catalyst.

10. The polymer composition according to claim 9, comprising (A) 35 to 55 weight percent of an ethylene / silane copolymer; (B) 15 wt % to 35 wt % of a flame retardant, wherein the flame retardant is TDS having a structure of formula (1); (C) 10 to 20 weight percent of a first flame retardant synergist, wherein the first flame retardant synergist is antimony trioxide; (D) 1 to 10 weight percent of a second flame retardant synergist, wherein the second flame retardant synergist is zinc oxide; (E) greater than 0 wt % to 7 wt % of a moisture cure catalyst; (F) from greater than 0 wt% to 7 wt% of a second polyolefin, the second polyolefin being an ethylene-based polymer; and (G) greater than 0 wt % to 0.5 wt % of an antioxidant; The aggregate of components (A) to (G) accounts for 100% by weight of the polymer composition.

11. A cable, comprising: conductor; and A coating on the conductor, the coating comprising Silane functionalized polyolefins; and Flame retardant, the flame retardant is tetrabromophthalic anhydride diamine siloxane (TDS) having the structure of formula (1) Formula (1) wherein n is an integer from 1 to 40; and Each R is the same or different, and each R is independently selected from hydrogen and C1-C 20 A group consisting of hydrocarbon groups.