Crosslinkable compositions based on organosilicon compounds

By using an organic silicon compound in the RTV1 sealing compound with a condensation reaction of a heterocyclic compound and a silicone, a crosslinkable composition containing a partial hydrolyzate is formed, and a long processing time, yellowing and poor stability in the prior art is solved. Problem, rapid curing and high stability are achieved, the ratio of cleavage products and catalysts of toxicology concerns, and the ability to adjust the surface drying time and modulus.

CN118974157APending Publication Date: 2024-11-15WACKER CHEMIE AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094396.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing RTV1 sealing compounds are processed in hard variants for too long, and the use of organotin catalysts can lead to undesirable yellowing, and are difficult to maintain stability in warm and humid environments, and are difficult to control the surface drying time and tensile stress values. .

Method used

By using an organosilicon compound having at least two OH groups with the condensation reaction of a specific heterocyclic compound and a siloxane component, a crosslinkable composition containing a partial hydrolysate is formed, the use of an organotin catalyst is avoided, and by adjusting the group Particularly proportional and additives to control curing properties.

Benefits of technology

It realizes fast curing, high stability and good deformation resistance at room temperature, avoids the use of organic tin catalysts, reduces the proportion of cleavage products and catalysts that are concerned by toxicology, and can adjust the surface drying time within the margin and modulus.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005065166710000271
    Figure BDA0005065166710000271
Patent Text Reader

Abstract

The present invention relates to crosslinkable compositions based on organosilicon compounds which cure to form highly stable materials while removing alcohols. These compositions can be produced using (A) organosilicon compounds having at least two OH groups, (B) heterocyclic compounds of the formula A [CR12SiRa (OR2) 3-a] x (I) and / or their partial hydrolysates and (C) at least one compound containing units of the formula Si (OR4) 3O1 / 2 (III), Si (OR4) 2O2 / 2 (IV), (OR4) SiO3 / 2 (V) and optionally SiO4 / 2 (VI), the groups and indices having the meanings indicated in claim 1, with the proviso that compound (C) contains at least 10 mol% of the units of formula (V). The invention also relates to a method for the production thereof and to the use thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to crosslinkable compositions based on organosilicon compounds which cure with elimination of alcohols to give materials having very high stability, to a process for their production and to their use. Background Art

[0002] One-component sealing compounds are known which are storable with exclusion of water and which cure at room temperature upon ingress of water with elimination of the alcohol to produce an elastomer. These products are used in large quantities, for example in the construction industry. These mixtures are based on polymers terminated by silyl groups with active substituents, such as OH groups or hydrolyzable groups, such as alkoxy groups. In addition, these sealing compounds may contain fillers, plasticizers, crosslinking agents, catalysts and various additives.

[0003] The catalysts used are often diorganotin compounds. In some cases, titanium compounds are also used. However, titanium catalysts lead to undesirable yellowing very quickly and are therefore not preferred.

[0004] However, from the point of view of chemical legislation, the preferred organotin compounds are the subject of increasingly critical classifications. Therefore, attempts have been made to use substances such as dioctyltin and dibutyltin compounds in RTV1 sealing compounds in smaller amounts or even no longer at all.

[0005] EP 2 176 351 B1 teaches the production of RTV1 sealing compounds based on 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine. The examples cited show that it is also possible to completely dispense with the use of organotin catalysts. However, in this case, in the case of the hard variants, the processing times are too long to be used as joint sealants.

[0006] EP 2 855 591 B1 describes the addition of hydrolysis products formed from unsubstituted alkyltrialkoxysilanes to produce RTV1 sealing compounds based on 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine. These specific siloxanes improve the resistance of the cured composition to the effects of warm and humid ambient conditions. The composition contains a dialkyltin compound as a catalyst.

[0007] EP 3 433 321 B1 describes the production of a removable RTV1 coating composition based on N,N-dialkylaminomethyltrialkoxysilane. As well as other ingredients, the mixture also contains a partial hydrolyzate formed from tetraethoxysilane. The composition is selected so that the cured material has good adhesion to various substrates. Due to the high activity of the selected α-silane, no additional catalyst or curing accelerator is required.

[0008] It has surprisingly been found that RTV1 sealing compounds based on 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine (even without added organotin catalysts) have very good curing characteristics when these compositions contain partial hydrolysates of tetraalkoxysilanes. Due to the relatively low activity of the partial hydrolysates, for example, the person skilled in the art could not expect to shorten the skin time of RTV1 sealing compounds based on α-silanes in a controlled manner.

[0009] What is particularly surprising here is that the cured material has low tensile stress values ​​under strain.

[0010] Furthermore, it is very particularly surprising that the cured material has low tensile stress values ​​under strain when only small amounts of plasticizer are used. Summary of the invention

[0011] The present invention provides compositions which are crosslinkable by condensation reaction and can be produced using:

[0012] (A) an organosilicon compound having at least two OH groups,

[0013] (B) a heterocyclic compound of the formula:

[0014] A[CR 1 2SiR a (OR 2 ) 3-a ] x (I)

[0015] in

[0016] A represents heterocyclic AH x and contains at least one ring-forming element of the 3rd and / or 5th main groups, wherein x hydrogen atoms are bonded to CR 1 2 groups, wherein at least one of these bonds is present on a ring-forming element of the 3rd or 5th main group,

[0017] R represents identical or different, monovalent, optionally substituted hydrocarbon groups,

[0018] R 1 may be the same or different and represent a hydrogen atom or a monovalent, optionally substituted hydrocarbon group, R 2 may be the same or different and represent a monovalent, optionally substituted hydrocarbyl group,

[0019] a = 0 or 1, preferably 0, and

[0020] x=1, 2 or 3, preferably 1 or 2, more preferably 1,

[0021] and / or its partial hydrolysate

[0022] as well as

[0023] (C) at least one compound containing a unit of the formula

[0024] Si(OR 4 )3O 1 / 2 (III)

[0025] Si(OR 4 )2O 2 / 2 (IV),

[0026] (OR 4 )SiO 3 / 2 (V) and

[0027] Optionally

[0028] SiO 4 / 2 (VI)

[0029] in

[0030] R 4 may be the same or different and are independently in each case an alkyl group,

[0031] Provided that compound (C) contains at least 10 mol % of units of formula (V).

[0032] The partial hydrolysates of compounds of formula (I) may be partial homohydrolysates or partial cohydrolysates. If component (B) used according to the invention contains partial hydrolysates of compounds of formula (I), preference is given to those having up to 10 silicon atoms.

[0033] The radical R is preferably an optionally substituted monovalent hydrocarbon radical having 1 to 18 carbon atoms, more preferably an alkyl radical, a vinyl radical, a 3,3,3-trifluoroprop-1-yl radical and a phenyl radical, especially a methyl radical.

[0034] Examples of radicals R are alkyl radicals, such as methyl, ethyl, n-propyl, isopropyl, 1-n-butyl, 2-n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl radicals; hexyl radicals, such as n-hexyl radicals; heptyl radicals, such as n-heptyl radicals; octyl radicals, such as n-octyl radicals and isooctyl radicals, such as 2,2,4-trimethylpentyl radicals; nonyl radicals, such as n-nonyl radicals; decyl radicals, such as n-decyl radicals; dodecyl radicals, such as n-decyl radicals; dialkyl groups; octadecyl groups such as n-octadecyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, cycloheptyl and methylcyclohexyl groups; alkenyl groups such as vinyl, 1-propenyl and 2-propenyl groups; aryl groups such as phenyl, naphthyl, anthracenyl and phenanthrenyl groups; alkylaryl groups such as o-, m-, p-tolyl groups; xylyl groups and ethylphenyl groups; and aralkyl groups such as benzyl groups and α- and β-phenylethyl groups.

[0035] Examples of substituted radicals R are halogenated alkyl radicals such as 3,3,3-trifluoroprop-1-yl radical, 1,1,1,3,3,3-hexafluoroprop-2-yl radical and heptafluoroprop-2-yl radical, halogenated aryl radicals such as o-, m- and p-chlorophenyl radicals, and 2-methoxyethyl radical, 2-methoxyprop-1-yl radical and 2-(2-methoxyethoxy)ethyl radical.

[0036] Group R 1 Examples of are a hydrogen atom and the groups specified for R.

[0037] Group R 1 Preference is given to hydrogen atoms and hydrocarbyl groups having 1 to 20 carbon atoms, especially hydrogen atoms.

[0038] Group R 2 Examples of are the groups specified for R.

[0039] Group R 2 Preference is given to alkyl groups having 1 to 6 carbon atoms, more preferably methyl and ethyl groups, especially ethyl groups.

[0040] Group A is a cyclic compound having ring-forming atoms of at least two different elements, provided that at least one of the ring-forming atoms is a -CR 1 2-An element of the 3rd and / or 5th main group at the bonding site of the carbon atom of the group.

[0041] The radical A is preferably a cyclic organic compound whose ring structure, as well as the carbon atoms, also contains at least one element of main group 3 and / or main group 5 and more preferably at least one further heteroatom.

[0042] The term "heteroatom" is understood hereinafter to mean all ring-forming atoms other than carbon.

[0043] The ring-forming heteroatoms in group A are preferably nitrogen, phosphorus, oxygen, silicon and sulfur, more preferably nitrogen and oxygen.

[0044] The group A may also be an optionally substituted, saturated or partially unsaturated heterocycle. If the ring A is substituted, the substituents are preferably halogen atoms, hydrocarbon groups and organoxy groups, wherein these substituents may be polyvalent groups which may be bonded to one or more ring-forming atoms.

[0045] The radical A may also contain ring carbon atoms which have an oxygen or sulfur atom bonded via a double bond, provided that such ring carbon atoms do not have a carbon atom which is bonded to the CR radical of formula (I). 1 Any direct bond to a ring-forming heteroatom of the 3rd or 5th main group of the 2 group.

[0046] The group A may also include ring carbon atoms having nitrogen or phosphorus atoms bonded via a double bond, but this is not preferred.

[0047] The radical A is preferably a 3-, 4-, 5-, 6-, 7- or 8-membered heterocycle which, as ring atoms, has, in addition to carbon, nitrogen and / or phosphorus and / or oxygen and / or sulfur as heteroatoms, provided that at least one ring atom is an element of main group 3 and / or main group 5, wherein further rings may also be connected by fusion.

[0048] More preferably, the heterocycle on which the A group is based is a 5- and 6-membered heterocycle which contains further ring heteroatoms and heteroatoms from main group 3 and / or main group 5 which are bound to CR of the compound of formula (I). 1 2 groups required.

[0049] Examples of heterocycles on which the A group is based are aziridine, azetidine, pyrrole, pyrrolidine, 1,3-oxazolidine, 1,3-thiazolidine, 1H-1,2-oxadiazole, Δ 2 -1,2-diazoline, Δ 4 -1,2-oxadiazole, 1,3-oxadiazole, Δ 2 -1,3-diazoline, Δ 4 -1,3-oxadiazolidine, 1,3-oxadiazolidine, 1,2,3-triazole, 1,2,4-triazole, tetrazole, Δ 4-1,2-diazolin-3-one, piperidine, tetrahydro-1,4-oxazine, tetrahydro-1,4-thiazine, hexahydro-1,3-diazine, hexahydro-1,4-diazine, 1-methylhexahydro-1,4-diazine, hexahydro-1,3,5-triazine, hexahydro-1,3-diazine-4-one, 4-methylhexahydro-1,4-diazine-3-one, 1H-azepine, hexahydroazepine, octahydroazine, 1H-benzo[b]pyrrole, 2,3-dihydrobenzo[b]pyrrole, 9H-dibenzopyrrole, benzo[d]-1,2-diazine, benzo[d]-1,3-diazine and benzo[d]-1,2,3-triazole.

[0050] Particular preference is given to pyrrolidine, piperidine, tetrahydro-1,4-oxazine, tetrahydro-1,4-thiazine, tetrahydro-1,4-diazine and 1-methyltetrahydro-1,4-diazine, especially tetrahydro-1,4-oxazine.

[0051] Examples of the heterocyclic compound (B) are

[0052] 1-(Triethoxysilylmethyl)aziridine, 1-(Triethoxysilylmethyl)azetidine, 1-(Triethoxysilylmethyl)pyrrole, 1-(Triethoxysilylmethyl)pyrrolidine, 3-(Triethoxysilylmethyl)-1,3-oxazolidine, 3-(Triethoxysilylmethyl)-1,3-thiazolidine, 1-(Triethoxysilylmethyl)-1H-1,2-oxadiazole, 1-(Triethoxysilylmethyl)-Δ 2 -1,2-oxadiazolidine, 1-(triethoxysilylmethyl)-Δ 4 -1,2-oxadiazole, 1-(triethoxysilylmethyl)-1,3-oxadiazole, 1-(triethoxysilylmethyl)-Δ 2 -1,3-oxadiazolidine, 1-(triethoxysilylmethyl)-Δ 4 -1,3-oxadiazolidine, 1-(triethoxysilylmethyl)-1,3-oxadiazolidine, 1,3-bis(triethoxysilylmethyl)-1,3-oxadiazolidine, 1-(triethoxysilylmethyl)-1H-1,2,3-triazole, 2-(triethoxysilylmethyl)-2H-1,2,3-triazole, 1-(triethoxysilylmethyl)-1H-1,2,4-triazole, 4-(triethoxysilylmethyl)-4H-1,2,4-triazole, 1-(triethoxysilylmethyl)-1H-tetrazole, 2-(triethoxysilylmethyl)-2H-tetrazole, 1-(triethoxysilylmethyl)-Δ 4-1,2-diazolin-3-one, 1-(triethoxysilylmethyl)piperidine, 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine, 4-(1-(triethoxysilyl)ethyl)tetrahydro-1,4-oxazine, 4-(2-(triethoxysilyl)prop-2-yl)tetrahydro-1,4-oxazine, 4-(1-phenyl-1-(triethoxysilyl)ethyl)tetrahydro-1,4-oxazine, 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine Thiazine, 1-(triethoxysilylmethyl)hexahydro-1,3-diazine, 1-(triethoxysilylmethyl)hexahydro-1,4-diazine, 1-methyl-4-(triethoxysilylmethyl)hexahydro-1,4-diazine, 1,4-bis(triethoxysilylmethyl)hexahydro-1,4-diazine, 1,4-bis(1-(triethoxysilyl)ethyl)hexahydro-1,4-diazine, 1-(triethoxysilylmethyl)hexahydro-1,3,5-triazine, 1,3- Bis(triethoxysilylmethyl)hexahydro-1,3,5-triazine, 1,3,5-tris(triethoxysilylmethyl)hexahydro-1,3,5-triazine, 1-(triethoxysilylmethyl)hexahydro-1,3-diazine-4-one, 1-(triethoxysilylmethyl)-4-methylhexahydro-1,4-diazine-3-one, 1-(triethoxysilylmethyl)-1H-azepine, 1-(triethoxysilylmethyl)hexahydroazepine, 1-(triethoxymethyl 1-(triethoxysilylmethyl)benzo[d]-1,2-oxadiazole, 1-(triethoxysilylmethyl)benzo[d]-1,3-oxadiazole and 1-(triethoxysilylmethyl)benzo[d]-1,2,3-triazole.

[0053] Further examples are all of the abovementioned compounds in which the triethoxysilyl group has been replaced by a trimethoxysilyl group, a diethoxymethylsilyl group or a dimethoxymethylsilyl group.

[0054] The heterocyclic compounds (B) used according to the invention are standard commercially available compounds or can be prepared by standard chemical methods.

[0055] The composition of the invention contains component (B) in an amount of preferably 0.1 to 30 parts by weight, more preferably 0.5 to 20 parts by weight, in particular 1 to 10 parts by weight, based in each case on 100 parts by weight of component (A).

[0056] The organosilicon compound (A) used according to the invention may be any organosilicon compound having at least two OH groups which has hitherto also been used in compositions crosslinkable by condensation reactions.

[0057] The organosilicon compounds (A) used according to the invention are preferably those containing units of the formula 3 b (OH) c SiO (4-b-c) / 2 (II)

[0058] in

[0059] R 3 may be identical or different and represent an optionally substituted hydrocarbyl group which may be interrupted by an oxygen atom,

[0060] b is 0, 1, 2 or 3, preferably 2, and

[0061] c is 0, 1, 2 or 3, preferably 0 or 1,

[0062] The proviso is that the sum of b+c is ≤3 and that at least two condensable OH groups are present in each molecule.

[0063] Group R 3 Preferred are monovalent hydrocarbon groups having 1 to 18 carbon atoms and optionally substituted by halogen atoms, amino groups, ether groups, ester groups, epoxy groups, mercapto groups, cyano groups or (poly) glycol groups, the latter being formed from oxyethylene and / or oxypropylene units, more preferably alkyl groups having 1 to 12 carbon atoms, in particular methyl groups.

[0064] Group R 3 Examples are the examples given for the R group.

[0065] More preferably, the organosilicon compounds (A) used according to the invention are essentially linear, OH-terminated organopolysiloxanes, especially α,ω-dihydroxydialkylpolysiloxanes.

[0066] An example of an organosilicon compound (A) is (HO)Me2SiO[SiMe2O] 30-2000 SiMe2(OH), where Me = methyl group.

[0067] The organosilicon compounds (A) used according to the invention preferably have a viscosity of in each case 10 3 Up to 10 6 mPas, more preferably 10 4 To 350000mPas.

[0068] The organosilicon compounds (A) are commercial products or can be prepared by standard methods in silicon chemistry.

[0069] Group R 4 Examples of are independently the examples given above for the radical R.

[0070] Group R 4 Preferred is an alkyl group having 1 to 4 carbon atoms, more preferably a methyl group or an ethyl group.

[0071] The compounds (C) used according to the invention contain units of the formulae (III), (IV) and (V) in a total amount of preferably at least 70 mol %, more preferably at least 85 mol % and in particular at least 90 mol %.

[0072] The compounds (C) used according to the invention contain at least 10 mol %, preferably 10 mol % to 50 mol % and more preferably 12 mol % to 30 mol % of units of the formula (V).

[0073] The compounds (C) used according to the invention preferably contain 15 to 60 mol % of units of the formula (III).

[0074] The compounds (C) used according to the invention preferably contain 20 to 60 mol % of units of the formula (IV).

[0075] The compounds (C) used according to the invention preferably contain 10 to 50 mol % of units of the formula (V), 15 to 60 mol % of units of the formula (III) and 20 to 60 mol % of units of the formula (IV).

[0076] The compounds (C) used according to the invention may, in addition to the units of the formulae (III), (IV) and (V), also contain units of the formula (VI), which is not preferred.

[0077] If the compounds (C) used according to the invention contain units of the formula (VI), preferably less than 2 mol % of these units.

[0078] Preferably, the compounds (C) used according to the invention consist of units of the formulae (III), (IV) and (V) and optionally (VI).

[0079] Although not represented by formulae (III) to (VI), the compound (C) used according to the present invention may contain up to 1% by weight of residual Si-OH as an impurity as a result of the preparation.

[0080] Examples of siloxanes (C) used according to the invention are

[0081] (Si(OEt)2O 2 / 2 )0.42 (Si(OEt)O 3 / 2 ) 0.19 (Si(OEt)3O 1 / 2 ) 0.39 , wherein Mw=1000 g / mol, Mn=800 g / mol and Mw / Mn=1.2, and

[0082] (Si(OEt)2O 2 / 2 ) 0.47 (Si(OEt)O 3 / 2 ) 0.35 (Si(OEt)3O 1 / 2 ) 0.16 (SiO 4 / 2 ) 0.02 , wherein Mw = 1400 g / mol, Mn = 900 g / mol and Mw / Mn = 1.6.

[0083] Siloxane (C) has a weight average Mw of preferably 500 to 10000 g / mol, more preferably 500 to 8000 g / mol.

[0084] Siloxane (C) has a number average Mn of preferably 200 to 5000 g / mol, more preferably 200 to 3000 g / mol.

[0085] Siloxane (C) has a polydispersity Mw / Mn of preferably 1-5, more preferably 1-4.

[0086] In the present invention, the weight average Mw and the number average Mn are determined according to DIN 1333: 1992-02 Part 4, rounded to the nearest hundred, by gel permeation chromatography (GPC or size exclusion chromatography (SEC)) according to DIN 55672-1 using polystyrene standards and a refractive index detector (RI detector). Unless otherwise specified, THF is used as eluent for phenyl-containing components and toluene is used as eluent for phenyl-free components, and the analysis is carried out at a column temperature of 45° C. The polydispersity is the quotient of Mw / Mn.

[0087] The organosiloxane (C) is preferably liquid at 25° C. and 1000 hPa.

[0088] The siloxanes (C) used according to the invention are commercially available, for example under the name Siloxane® from WackerChemie AG, Munich, Germany. TES 40, or can be prepared by standard methods in silicon chemistry. For example, the compounds (C) used according to the invention can be prepared by hydrolysis of tetraalkoxysilanes and subsequent condensation.

[0089] The composition of the present invention contains component (C) in an amount of preferably 1 to 20 parts by weight, more preferably 4 to 10 parts by weight, based in each case on 100 parts by weight of component (A).

[0090] In addition to components (A), (B) and (C), the composition of the invention can then contain all substances which have hitherto also been used in compositions crosslinkable by condensation reactions, for example catalysts (D), compounds containing basic nitrogen (E), fillers (F), adhesion promoters (G), plasticizers (H), further crosslinkers (J), additives (K) and solvents (L), wherein components (J), (E) and (G) are different from components (B) and (C) and component (L) is different from the plasticizer (H).

[0091] Examples of the catalyst (D) are known titanium compounds such as tetraisopropoxytitanate, zirconium compounds and hafnium compounds, and metal carboxylates such as zinc (2-ethylhexanoate) and octylphosphonic acid or its derivatives.

[0092] Any catalyst (D) used is preferably an alkoxide of a metal of the fourth transition group of the Periodic Table of the Elements, a carboxylate of a metal of the twelfth transition group of the Periodic Table of the Elements, and a phosphonate, more preferably a titanium alkoxide, a zinc carboxylate and a derivative of octylphosphonic acid, in particular tetrabutyl titanate, zinc ethylhexanoate or octylphosphonate.

[0093] If the composition of the invention contains a catalyst (D), the amount thereof is preferably 0.0001 to 2 parts by weight, more preferably 0.001 to 1 part by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention preferably contains a catalyst (D).

[0094] The composition of the invention contains an organotin compound, preferably in an amount of not more than 0.01 part by weight, more preferably not more than 0.001 part by weight, based in each case on 100 parts by weight of the composition of the invention, wherein the composition of the invention in particular contains no organotin compound.

[0095] Any compound (E) containing a basic nitrogen used according to the invention is preferably selected from the group consisting of: a compound of the formula

[0096] NR 6 3(IX)

[0097] Where R 6 may be identical or different and are hydrogen atoms or hydrocarbon radicals which are optionally substituted by hydroxyl groups, halogen atoms, amino groups, ether groups, ester groups, epoxy groups, mercapto groups, cyano groups or polyglycol residues, the latter being formed from oxyethylene and / or oxypropylene units,

[0098] Provided that, in formula (IX), no more than two R 6 has the meaning of a hydrogen atom, wherein, if two or more R 6 , then these can also be connected to each other to form a ring structure,

[0099] and an organosilicon compound having at least one organic group and containing basic nitrogen, different from component (B), which consists of units of the formula:

[0100] R 7 k Y l Si(OR 8 ) m O (4-k-l-m) / 2 (X),

[0101] in,

[0102] R 7 may be the same or different and are monovalent, SiC-bonded organic groups that do not contain basic nitrogen,

[0103] R 8 may be the same or different and have a 2 Given the definition,

[0104] Y may be the same or different and is a monovalent, SiC-bonded, basic nitrogen-containing organic group,

[0105] k is 0, 1, 2, or 3,

[0106] l is 0, 1, 2, 3, or 4, and

[0107] m is 0, 1, 2, or 3,

[0108] The conditions are that the sum of k+l+m is not greater than 4 and that at least one group Y is present per molecule.

[0109] R 6 and R 7 Examples of radicals are in each case independently the examples given for R for optionally substituted hydrocarbyl radicals.

[0110] Optionally substituted hydrocarbon group R 6 Preferred are those having 1 to 18 carbon atoms.

[0111] Group R 7 Preference is given to hydrocarbon radicals having 1 to 18 carbon atoms, particular preference being given to methyl, ethyl and n-propyl radicals, especially to methyl radicals.

[0112] Group R 8An example is for the group R 2 Examples given.

[0113] Group R 8 Preferred are the methyl and ethyl groups.

[0114] Examples of the group Y are groups of the formula: H2NCH2-, H2N(CH2)2-, H2N(CH2)3-, H2N(CH2)2NH(CH2)2-, H2N(CH2)2NH(CH2)3-, H2N(CH2)2NH(CH2)2NH(CH2)3-, H3CNH(CH2)3-, C2H5NH(CH2)3-, H3CNH(CH2)2-, C2H5NH(CH2)2-, H2N(CH2)4-, H2N(CH2)5-, H(NHCH2CH2)3-, C4H9NH(CH2)2NH(CH2)2-, cyclo-C6H 11 NH(CH2)3-, cyclo-C6H 11 NH(CH2)2-, (CH3)2N(CH2)3-, (CH3)2N(CH2)2-, (C2H5)2N(CH2)3- and (C2H5)2N(CH2)2-.

[0115] Preferably, Y is H2N(CH2)3-, H2N(CH2)2NH(CH2)3-, H3CNH(CH2)3-, C2H5NH(CH2)3- and cyclo-C6H 11 NH(CH2)3- groups, with particular preference given to H2N(CH2)2NH(CH2)3- and cyclo-C6H 11 NH(CH2)3- group.

[0116] If the organosilicon compound composed of units of formula (X) is a silane, k is preferably 0, 1 or 2, more preferably 0 or 1, l is preferably 1 or 2, more preferably 1, and m is preferably 1, 2 or 3, more preferably 2 or 3, provided that the sum of k+l+m=4.

[0117] Examples of silanes of formula (X) which may be used according to the invention are H2N(CH2)3-Si(OCH3)3, H2N(CH2)3-Si(OC2H5)3, H2N(CH2)3-Si(OCH3)2CH3, H2N(CH2)3-Si(OC2H5)2CH3, H2N(CH2)2NH(CH2)3-Si(OCH3)3, H2N(CH2)2NH(CH2)3-Si(OC2H5)3, H2N(CH2)2NH(CH2)3-Si(OCH3)2CH3, H2N(CH2)2NH(CH2)3-Si(OC2H5)3, H2N(CH2)2NH(CH2)3-Si(OCH3)2CH3, H2N(CH2)2NH(CH2)3-Si(OC2H5)2CH3, H2N(CH2)2NH(CH2)3-Si(OC2H5)3, cyclo-C6H 11 NH(CH2)3-Si(OCH3)3, Cyclo-C6H 11 NH(CH2)3-Si(OC2H5)3, cyclo-C6H 11 NH(CH2)3-Si(OCH3)2CH3, cyclo-C6H 11 NH(CH2)3-Si(OC2H5)2CH3, HN((CH2)3-Si(OCH3)3)2 and HN((CH2)3-Si(OC2H5)3)2 and their partial hydrolysis products, preferably H2N(CH2)2NH(CH2)3-Si(OCH3)3, H2N(CH2)2NH(CH2)3-Si(OC2H5)3, H2N(CH2)2NH(CH2)3-Si(OCH3)2CH3, H2N(CH2)2NH(CH2)3-Si(OC2H5)2CH3, cyclo-C6H 11 NH(CH2)3-Si(OC2H5)3, cyclo-C6H 11 NH(CH2)3-Si(OCH3)2CH3 and cyclo-C6H 11 NH(CH2)3-Si(OC2H5)2CH3, and particularly preferred are H2N(CH2)2NH(CH2)3-Si(OC2H5)3, H2N(CH2)2NH(CH2)3-Si(OC2H5)2CH3, cyclo-C6H 11 NH(CH2)3-Si(OC2H5)3 and cyclo-C6H 11 NH(CH2)3-Si(OC2H5)2CH3 and their respective partial hydrolysis products.

[0118] If the organosilicon compound composed of units of formula (X) is an organopolysiloxane, the average value of k is preferably between 0.5 and 2.5, more preferably between 1.4 and 2.0, the average value of l is preferably between 0.01 and 1.0, more preferably between 0.01 and 0.6, and the average value of m is preferably between 0 and 2.0, more preferably between 0 and 0.2, provided that the sum of k, l and m is not greater than 3.

[0119] The organopolysiloxanes composed of units of the formula (X) which can be used according to the invention have a relative humidity of preferably 5 to 10 at 25° C. 5 mPas, more preferably 10 to 10 4 Viscosity in mPas.

[0120] Examples of organopolysiloxanes composed of units of formula (X) which can be used according to the invention are H2N(CH2)3-Si(OCH3)2-O-Si(CH3)(OCH3)2, H2N(CH2)3-Si(OC2H5)2-O-Si(CH3)(OCH3)2, H2N(CH2)3-Si(OC2H5)2-O-Si(CH3)(OC2H5)2, H2N(CH2)3-Si(OCH3)(CH3)-O-Si(CH3)(OCH3)2, H2N(CH2)3-Si(OCH3)(CH3)-O-Si(CH3)(OCH3)2, H2N(CH2)3-Si(OCH3)(CH3)-O-Si(OCH3)3, H2N(CH2)3-Si(OC2H5)(CH3)-O-Si(OCH3)3, H2N(CH2)2NH(CH2)3-Si(OCH3)2-O-Si(CH3)(OCH3)2 , H2N(CH2)2NH(CH2)3-Si(OC2H5)2-O-Si(CH3)(OCH3)2 , H2N(CH2)2NH(CH2)3-Si(OC2H5)2-O-Si(CH3)(OC2H5)2 , H2N(CH2)2NH(CH2)3-Si(OCH3)(CH3)-O-Si(CH3)(OCH3)2 , H2N(CH2)2NH(CH2)3-Si(OCH3)(CH3)-O-Si(OCH3)3 , H2N(CH2)2NH(CH2)3-Si(OC2H5)(CH3)-O-Si(OCH3)3 , Ring-C6H 11 NH(CH2)3-Si(OCH3)2-O-Si(CH3)(OCH3)2, cyclo-C6H 11 NH(CH2)3-Si(OC2H5)2-O-Si(CH3)(OCH3)2, Cyclo-C6H 11 NH(CH2)3-Si(OC2H5)2-O-Si(CH3)(OC2H5)2, Cyclo-C6H11 NH(CH2)3-Si(OCH3)(CH3)-O-Si(CH3)(OCH3)2, cyclo-C6H 11 NH(CH2)3-Si(OCH3)(CH3)-O-Si(OCH3)3 and cyclo-C6H 11 NH(CH2)3-Si(OC2H5)(CH3)-O-Si(OCH3)3, H2N(CH2)3-Si(OCH3)2-(O-Si(CH3)2) 1-100 -O-Si(OCH3)2-(CH2)3NH2 、H2N(CH2)2NH(CH2)3-Si(OCH3)2-(O-Si(CH3)2) 1-100 -O-Si(OCH3)2-(CH2)3NH(C H2)2NH2 and cyclo-C6H 11 NH(CH2)3-Si(OCH3)2-(O-Si(CH3)2) 1-100 -O-Si(OCH3)2-(CH2)3NH-cyclo-C6H 11 and their partial hydrolysis products, with particular preference given to the partial hydrolysis products of H2N(CH2)3-Si(OC2H5)2-O-Si(CH3)(OC2H5)2.

[0121] Organosilicon compounds consisting of units of the formula (X) are commercial products or can be prepared by standard methods in silicon chemistry.

[0122] Examples of amines of the formula (IX) are cyclohexylamine, triethylamine, trioctylamine, butylamine, dodecylamine, diethyl-n-propylamine, cyclohexylmethylamine, 2-aminoethanol, 2-amino-n-propanol, 2-amino-2-methyl-1-propanol, 2-dimethylamino-2-methyl-1-propanol, N,N-diethylethanolamine, ethylenediamine, coconut amine, coconut methylamine, N,N-dimethylethanolamine and aniline.

[0123] If component (E) is used, it preferably contains an organosilicon compound consisting of units of the formula (X).

[0124] If the composition of the invention contains component (E), the amount thereof is preferably 0.001 to 10 parts by weight, more preferably 0.01 to 1 part by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention preferably contains component (E).

[0125] Any organosilicon compound (E) used according to the invention may also assume the function of a curing catalyst or cocatalyst in the composition of the invention.

[0126] Furthermore, any organosilicon compounds (E) used according to the invention may act as adhesion promoters and / or water scavengers.

[0127] Examples of fillers (F) are non-reinforcing fillers, ie, fillers having a molecular weight of up to 50 m 2 / g of fillers, such as quartz, diatomaceous earth, calcium silicate, zirconium silicate, zeolite, metal oxide powders, such as aluminum oxide, titanium oxide, iron oxide or zinc oxide or mixed oxides thereof, barium sulfate, calcium carbonate, gypsum, silicon nitride, silicon carbide, boron nitride, glass powder and polymer powders, such as polyacrylonitrile powder; reinforcing fillers, i.e., having a BET surface area of ​​more than 50 m 2 / g BET surface area of ​​fillers, such as fumed silica, precipitated silica, precipitated calcium carbonate, carbon black, such as furnace black and acetylene black, and mixed silica-alumina with a high BET surface area; fibrous fillers, such as asbestos and polymer fibers. The fillers mentioned may have been hydrophobized, for example by treatment with organosilanes or -siloxanes or by etherification of hydroxyl groups to alkoxy groups. If fillers (F) are used, they are preferably hydrophilic fumed silica, precipitated calcium carbonate and ground marble.

[0128] If the composition of the invention contains component (F), the amount thereof is preferably 1 to 80 parts by weight, more preferably 5 to 65 parts by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention preferably contains component (F).

[0129] Any adhesion promoter (G) used in the composition of the present invention may be silanes and organopolysiloxanes having functional groups, such as those having glycidoxypropyl, ureidopropyl or methacryloxypropyl groups. Examples of adhesion promoters (G) are epoxysilanes, such as glycidoxypropyltrimethoxysilane, glycidoxypropylmethyldimethoxysilane, glycidoxypropyltriethoxysilane or glycidoxypropylmethyldiethoxysilane, tris[3-(trimethoxysilyl)propyl]isocyanurate, 2-(3-triethoxysilylpropyl)maleic anhydride, N-(3-trimethoxysilylpropyl)urea, N-(3-triethoxysilylpropyl)urea, N-(trimethoxysilylmethyl)urea, N-(methyldimethoxysilylmethyl)urea, N-(3-triethoxysilylmethyl)urea, N-(3-methyldiethoxysilylmethyl)urea, O-methylcarbamate, methyldimethoxysilane, and methyldimethoxysilane. O-methyl-methyldimethoxysilane), O-methylcarbamate-methyl-trimethoxysilane, O-ethylcarbamate-methyl-methyldiethoxysilane, O-ethylcarbamate-methyl-triethoxysilane, 3-methacryloxypropyl-trimethoxysilane, methacryloxymethyl-trimethoxysilane, methacryloxymethyl-methyldimethoxysilane, methacryloxymethyl-triethoxysilane, methacryloxymethyl-methyldiethoxysilane, 3-acryloxypropyl-trimethoxysilane, acryloxymethyl-trimethoxysilane, acryloxymethyl-methyldimethoxysilane, acryloxymethyl-triethoxysilane and acryloxymethyl-methyldiethoxysilane and partial condensates thereof.

[0130] If the composition of the invention contains component (G), its amount is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 2.5 parts by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention, except when calcium carbonate is used as filler, preferably does not contain any component (G). If the composition of the invention contains calcium carbonate as filler (F), component (G) is preferably used.

[0131] Examples of plasticizers (H) are room temperature liquid dimethylpolysiloxanes having ends capped with trimethylsiloxy groups, especially having a viscosity in the range of 5 to 10 000 mPas at 25° C., and high boiling hydrocarbons, such as paraffin oil or mineral oil, which consists of cycloalkane and paraffin units.

[0132] If the composition of the invention contains component (H), the amount thereof is preferably 1 to 50 parts by weight, more preferably 10 to 35 parts by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention preferably contains component (H).

[0133] Any additional crosslinking agent (J) used in the composition of the present invention may be any crosslinking agent known hitherto having at least three condensable groups, for example a silane having at least three organooxy groups different from component (B).

[0134] Any additional crosslinking agent (J) used in the composition of the present invention is preferably a silane crosslinking agent, such as methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, 1,2-bis(trimethoxysilyl)ethane or 1,2-bis(triethoxysilyl)ethane and partial hydrolysis products thereof.

[0135] The further crosslinkers (J) used are more preferably partial hydrolysates of alkyltrialkoxysilanes, very particularly preferably partial hydrolysates of methyltrimethoxysilane.

[0136] Any additional crosslinking agents (J) used in the composition of the invention are commercial products or can be prepared by methods known in silicon chemistry.Partial hydrolysates of methyltrimethoxysilane are commercially available, for example, from WackerChemie AG, Munich, Germany, under the trade name TRASIL.

[0137] If the composition according to the invention contains a further crosslinker (J), the amount thereof is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, even more preferably 0.5 to 3 parts by weight, based in each case on 100 parts by weight of the composition according to the invention. The composition according to the invention preferably contains a crosslinker (J).

[0138] Examples of additives (K) are pigments, dyes, odorants, oxidation inhibitors, agents for influencing electrical properties such as conductive carbon black, flame retardants, light stabilizers and skin time extenders such as silanes with SiC-bonded mercaptoalkyl groups, cell generators such as azodicarbonamide, heat stabilizers and thixotropic agents such as polyethers, biocides such as fungicides, bactericides, acaricides, modulus regulators such as polydimethylsiloxanes having only one OH terminal group, and storage stability improvers such as alkylphosphonic acids.

[0139] If the composition of the invention contains component (K), the amount thereof is preferably 0.0001 to 10 parts by weight, more preferably 0.001 to 10 parts by weight, based in each case on 100 parts by weight of the composition of the invention. The composition of the invention preferably contains component (K).

[0140] Examples of solvents (L) are toluene, xylene, ethanol and methanol. These may be present as impurities in one or more of the components (A) to (K), for example due to production, or may be added intentionally, for example when component (C) is used as a solvent mixture.

[0141] If the composition according to the invention contains a solvent (L), the amount thereof is preferably 0.01 to 2 parts by weight, more preferably 0.1 to 1 part by weight, based in each case on 100 parts by weight of the composition according to the invention. The composition according to the invention preferably does not contain any solvent (L).

[0142] The compositions of the present invention are preferably those that can be produced using

[0143] (A) an organosilicon compound containing a unit of formula (II),

[0144] (B) a compound of formula (I),

[0145] (C) compounds containing units of the formulae (III), (IV) and (V) in a total amount of at least 80 mol %, provided that they contain at least 10 mol % of units of the formula (V),

[0146] Optionally, (D) a catalyst,

[0147] Optionally, (E) a basic nitrogen-containing compound,

[0148] Optionally, (F) filler,

[0149] Optionally, (G) an adhesion promoter,

[0150] Optionally, (H) a plasticizer,

[0151] Optionally, (J) an additional cross-linking agent,

[0152] Optionally, (K) additives, and

[0153] Optionally, (L) a solvent.

[0154] Furthermore, the compositions of the present invention are preferably those that can be produced using

[0155] (A) a substantially linear, OH-terminated organopolysiloxane,

[0156] (B) compounds of the formula (I) in which the heterocycle on which the radical A is based is pyrrolidine, piperidine, tetrahydro-1,4-oxazine, tetrahydro-1,4-thiazine, tetrahydro-1,4-diazine and 1-methyltetrahydro-1,4-diazine, in particular tetrahydro-1,4-oxazine,

[0157] (C) compounds containing units of the formulae (III), (IV) and (V) in a total amount of at least 90 mol %, provided that they contain from 12 mol % to 30 mol % of units of the formula (V),

[0158] Optionally, (D) a catalyst,

[0159] (E) a compound containing basic nitrogen,

[0160] Optionally, (F) filler,

[0161] Optionally, (G) an adhesion promoter,

[0162] Optionally, (H) a plasticizer,

[0163] Optionally, (J) an additional cross-linking agent,

[0164] Optionally, (K) additives, and

[0165] Optionally, (L) a solvent.

[0166] More preferably, the composition of the present invention is produced without using ingredients other than components (A) to (L).

[0167] The individual components of the composition of the present invention may each be one type of such component, or a mixture of at least two different types of such component.

[0168] To prepare the composition of the invention, all ingredients can be mixed with one another in any order. This mixing can be carried out at room temperature and ambient atmospheric pressure, i.e., about 900 to 1100 hPa, or under reduced pressure of about 20 hPa to 800 hPa. However, if desired, this mixing can alternatively be carried out at a higher temperature, for example at a temperature in the range of from 35° C. to 135° C. If desired, heating or cooling can be performed.

[0169] The invention further provides a process for producing the composition of the invention by mixing the individual components in any order.

[0170] The mixing of the individual components of the invention is preferably carried out with substantial exclusion of water from the surrounding atmosphere, which can be achieved, for example, by blanketing with dry air.

[0171] The component (C) used according to the invention can be mixed in at any time, for example before the addition of the compound (B) to the organosilicon compound (A), before or after the addition of the filler (F) or as the last component, in each case also before or after degassing. Preference is given to adding before the filler (F).

[0172] The order in which polymer, crosslinker and plasticizer are mixed is not important. For reasons of ease of processing, it is preferred to first form the initial charge from polymer (A) and optionally plasticizer (H), then add component (B) and optionally crosslinker (J), and then preferably component (C).

[0173] If filler (F) is added, preferably component (A), component (B), component (C), optional component (J) and optional component (E) are intimately mixed with one another before adding filler (F), preferably hydrophilic silica.

[0174] Preferably, if component (E) is used, the ratio of (E) to (F) is chosen such that for each square meter of BET surface area of ​​filler (F), at least 0.2 μmol of basic nitrogen-containing compound (E) is used.

[0175] If fillers (F) and plasticizers (H) are added, the mixture of polymer (A), plasticizer (H), component (C) and component (B) and optionally crosslinker (J) is intimately mixed by stirring.

[0176] If a hydrophilic fumed silica is added as filler (F), preference is given to intimately mixing component (A), plasticizer (H), component (C), component (B) and optionally component (J) before the addition of filler (F) until at least 90% of the OH groups of the organosilicon compound (A) have reacted with components (B) and (J), wherein component (E) is added at any time before the addition of the fumed silica. The ratio of (E) to (F) is preferably selected such that 0.2 μmol of basic nitrogen-containing compound (E) is used per square meter of BET surface area of ​​the filler.

[0177] In addition, the time point of adding the catalyst (D) is usually unimportant. However, it is wise to add the catalyst only at the end, because the mixture is then activated. Those skilled in the art generally wish to avoid the excessive mixing of already very reactive sealing compounds, because it is difficult or at least uneconomical to completely exclude moisture in the production of the mixture. Sometimes it is even necessary to keep the catalyst from contacting the polymer-crosslinker mixture that still contains a relatively large amount of unconverted OH groups, because then sometimes premature crosslinking of the mixture can occur. For this reason as well, those skilled in the art will avoid adding the catalyst too early. As an exception, those skilled in the art will add a crosslinking catalyst at the beginning of the mixture production, only when it is also a catalyst for the reaction of the OH polymer with the crosslinker.

[0178] The mixing of the ingredients may be interrupted at any point in time for any amount of time. In particular, it is preferred that the interruption be at least about 1 minute after the organosilicon compound (A) has been mixed with the compound (B) and any component (E) / any crosslinking agent (J), preferably with component (C) being added only after the interruption.

[0179] After all required ingredients have been mixed, the mixture is preferably degassed and introduced into a moisture-proof container.

[0180] The inventive production of the crosslinkable compositions of the invention can be carried out batchwise or continuously.

[0181] In a continuous process, preference is given to first mixing the organosilicon compound (A) with the compound (B) and any plasticizer (H) in a continuous manner, preferably using a dynamic mixer, wherein the reaction time of the organosilicon compound (A) with the compound (B) is from 1 to 60 minutes before any further mixture components are mixed. For example, the reaction time can be adjusted by controlled design of the pipeline length and pipeline cross section in the continuous system. The reaction time in the continuous process of the invention is preferably such that at least 90% of the OH groups of the organosilicon compound (A) have reacted with the compound (B). Subsequently, a static mixer can be used, for example, to continuously mix the organosilicon compound (C) of the invention and any crosslinking agent (J), the compound containing basic nitrogen (E), the adhesion promoter (G) and the plasticizer (H).

[0182] If desired, thereafter, preferably without intermediate storage, a filler (F), such as finely divided silicon dioxide, is mixed in continuously, for which it is possible to use, for example, a mixer with a rotor / stator system.

[0183] Before the possible addition of catalyst (D) and additives (K), the composition according to the invention can be degassed continuously, for example, by means of a twin-screw extruder.

[0184] The compositions of the invention are preferably one-component compositions which are storable with exclusion of water and cure on entry of water and are generally referred to in the specialist field as RTV-1 compositions.

[0185] The normal water content of air is sufficient for the crosslinking of the composition according to the invention. The composition according to the invention is preferably crosslinked at room temperature. If desired, this can also be carried out at a temperature higher or lower than room temperature, for example at -5°C to 15°C or at 30°C to 50°C, and / or with a water concentration that exceeds the normal water content of air.

[0186] The crosslinking is preferably carried out at a pressure of 100 to 1100 hPa, in particular at the pressure of the surrounding atmosphere.

[0187] The invention further provides shaped articles produced by crosslinking the compositions of the invention.

[0188] The compositions of the invention can be used for all end uses for which compositions which are storable with exclusion of water and which crosslink at room temperature on ingress of water to give elastomers can be used.

[0189] The compositions of the invention thus have excellent suitability, for example, as sealing compounds for joints, including vertical joints, and similar cavities, for example with a clear width of 10 to 40 mm, for example in buildings, land vehicles, ships and aircraft, or as adhesives or putties, for example in window construction or in the production of water baths or glass cabinets, and also, for example, for the production of protective coatings (including those for surfaces exposed to the constant action of fresh or sea water), or non-slip coatings, or elastomeric shaped articles, and for the insulation of electrical or electronic devices.

[0190] The compositions of the invention have the advantage that they are easy to produce and have a high storage stability over a long period of time.

[0191] The compositions of the invention have the advantage that they form only a small proportion, if any, of cleavage products of toxicological concern.

[0192] The compositions of the invention have the advantage that only small proportions, if any, of catalysts of toxicological concern are present.

[0193] The composition of the present invention has the advantage of having high resistance to deformation during processing.

[0194] The composition of the invention has the advantage that no readily visible spots are formed on the surface of the sealant when an aqueous smoothing agent is used.

[0195] Furthermore, the compositions according to the invention have the advantage that the open-air time can be adjusted within wide limits.

[0196] Furthermore, the compositions according to the invention have the advantage that they can be produced completely continuously.

[0197] Furthermore, the compositions of the invention have the advantage that variation of the type and proportion of compound (C) allows a controlled adjustment of the modulus of the cured composition within an extremely wide range. At the same time, the rheological properties of the uncured composition remain almost unchanged, which is generally desirable. DETAILED DESCRIPTION

[0198] In the examples described below, all viscosity values ​​are related to a temperature of 25° C. Unless otherwise stated, the following examples were conducted under the following conditions: ambient atmospheric pressure, i.e., about 1000 hPa, and room temperature, i.e., about 23° C., or the temperature determined when the reactants are mixed at room temperature without additional heating or cooling, and a relative humidity of about 50%. Furthermore, unless otherwise stated, all parts and percentage values ​​are based on weight.

[0199] The abbreviations used in the examples have the following meanings:

[0200] Me: methyl group

[0201] Et: ethyl group

[0202] Hydrolysis product (S1): 39 mol% of the formula Si(OEt)3O 1 / 2 units, 42 mol% of the formula Si(OEt)2O 2 / 2 units and 19 mol% of the formula (OEt)SiO 3 / 2 The hydrolysis product of oligomeric tetraethoxysilane composed of units.

[0203] Hydrolysis product (S2): 16 mol% of formula Si(OEt)3O 1 / 2 units, 47 mol% of the formula Si(OEt)2O 2 / 2 units, 35 mol% of the formula (OEt)SiO 3 / 2 The hydrolysis product of oligotetraethoxysilane composed of units of formula 1 and 2 mol % of units of formula Si(OEt)4.

[0204] Product (P): 16.0 mol% of the formula MeSi(OEt)2O 1 / 2 units, 46.4 mol% of the formula MeSi(OEt)O 2 / 2 units, 36.5 mol% of the formula MeSiO 3 / 2 units, 0.2 mol% of the formula Me2Si(OEt)O 1 / 2units and 0.9 mol% of the formula Me2SiO 2 / 2 The hydrolysis product of oligomeric silane composed of units.

[0205] Dry time:

[0206] For the purposes of the present invention, the expression "open time" defines the period of time before an elastic film is formed on a surface of a composition different from the underlying material. If the surface is touched, for example, with the tip of a pencil, no material sticks to it. Open times of more than 30 minutes are a clear indication that the desired rapid complete curing of the sealing compound has not been achieved.

[0207] Yield Point:

[0208] The yield point measurements were carried out with a rotational rheometer with air (MCR 301 Rheometer, from Anton Paar, Ostfildern-Scharnhausen, Germany). Before starting the measurement, the entire cartridge was subjected to a preliminary heat treatment for 3 hours at 25° C. in a climate-controlled cabinet. The measurement setup was as follows:

[0209] Temperature: 25℃

[0210] Measuring element: PP25

[0211] Gap distance: 0.2mm

[0212] Measuring method: Oscillation

[0213] Measurement: 5 times / decade (5per decade), every 10 seconds (every 10sec)

[0214] Shear stress: log 10Pa-10000Pa

[0215] Frequency: Constant 1Hz

[0216] The yield point corresponds to the interpolated shear stress in Pa at a loss factor of 1.

[0217] Comparative Example 1 (V1)

[0218] 300 g of α,ω-dihydroxypolydimethylsiloxane having a viscosity of 80000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Polymer FD 80"), 130 g of α,ω-bis(trimethylsiloxy)polydimethylsiloxane having a viscosity of 1000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Weichmacher 1000"), 9 g of 4-(triethoxysilylmethyl)-tetrahydro-1,4-oxazine, 5 g of the product (P), 11 g of 3-aminopropyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name of GF 93), 7 g of vinyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name An initial charge of 3.3 g of tetraethyl silicate (commercially available from Wacker Chemie AG, Munich, Germany, under the name "Silikat TES28") was mixed in a planetary mixer for a period of 30 minutes. Subsequently, 45 g of a 150 m 2 / g of fumed silica (commercially available from Wacker Chemie AG, Munich, Germany, under the name V15) and homogenize thoroughly under a pressure of 50 hPa.

[0219] The RTV1 composition thus obtained is dispensed into moisture-proof conventional polyurethane cartridges.

[0220] Example 1

[0221] 300 g of α,ω-dihydroxypolydimethylsiloxane having a viscosity of 80000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Polymer FD 80"), 130 g of α,ω-bis(trimethylsiloxy)polydimethylsiloxane having a viscosity of 1000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Weichmacher 1000"), 9 g of 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine, 5 g of the product (P), 11 g of 3-aminopropyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name of GF 93), 7 g of vinyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name An initial charge of 3.3 g of the hydrolyzate (S1) and 45 g of 150 m 2 / g of fumed silica (commercially available from Wacker Chemie AG, Munich, Germany, under the name V15) and homogenize thoroughly under a pressure of 50 hPa.

[0222] The RTV1 composition thus obtained is dispensed into moisture-proof conventional polyurethane cartridges.

[0223] Example 2

[0224] 300 g of α,ω-dihydroxypolydimethylsiloxane having a viscosity of 80000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Polymer FD 80"), 130 g of α,ω-bis(trimethylsiloxy)polydimethylsiloxane having a viscosity of 1000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Weichmacher 1000"), 9 g of 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine, 5 g of the product (P), 11 g of 3-aminopropyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name of GF 93), 7 g of vinyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name An initial charge of 3.3 g of the hydrolyzate (S1) and 45 g of 150 m 2 / g of fumed silica (commercially available from Wacker Chemie AG, Munich, Germany, under the name V15) are mixed in and thoroughly homogenized at a pressure of 50 hPa. Finally, 2.5 g of zinc(II) octoate are added and the mixture is homogenized again at a pressure of about 50 hPa (absolute) for 5 minutes.

[0225] The RTV1 composition thus obtained is dispensed into moisture-proof conventional polyurethane cartridges.

[0226] Example 3

[0227] 300 g of α,ω-dihydroxypolydimethylsiloxane having a viscosity of 80000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Polymer FD 80"), 130 g of α,ω-bis(trimethylsiloxy)polydimethylsiloxane having a viscosity of 1000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Weichmacher 1000"), 9 g of 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine, 5 g of the product (P), 11 g of 3-aminopropyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name of GF 93), 7 g of vinyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name An initial charge of 3.3 g of the hydrolyzate (S2) and 45 g of 150 m 2 / g of fumed silica (commercially available from Wacker Chemie AG, Munich, Germany, under the name V15) and homogenize thoroughly under a pressure of 50 hPa.

[0228] The RTV1 composition thus obtained is dispensed into moisture-proof conventional polyurethane cartridges.

[0229] Example 4

[0230] 300 g of α,ω-dihydroxypolydimethylsiloxane having a viscosity of 80000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Polymer FD 80"), 130 g of α,ω-bis(trimethylsiloxy)polydimethylsiloxane having a viscosity of 1000 mPa·s (commercially available from Wacker Chemie AG, Munich, Germany, under the name of "Weichmacher 1000"), 9 g of 4-(triethoxysilylmethyl)tetrahydro-1,4-oxazine, 5 g of the product (P), 11 g of 3-aminopropyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name of GF 93), 7 g of vinyltriethoxysilane (commercially available from Wacker Chemie AG, Munich, Germany, under the name An initial charge of 3.3 g of the hydrolyzate (S2) and 45 g of 150 m 2 / g of fumed silica (commercially available from Wacker Chemie AG, Munich, Germany, under the name V15) are mixed in and thoroughly homogenized at a pressure of 50 hPa. Finally, 2.5 g of zinc(II) octoate are added and the mixture is homogenized again at a pressure of about 50 hPa (absolute) for 5 minutes.

[0231] The RTV1 composition thus obtained is dispensed into moisture-proof conventional polyurethane cartridges.

[0232] Example 5

[0233] The mixtures produced in the examples and comparative examples were each spread onto a polyethylene film to produce a sheet having a thickness of 2 mm, from which the sheets were separated after one day of curing and suspended so as to be exposed to the air from all sides for a further 6 days, so that the samples were cured for a total of 7 days. The relative humidity was adjusted to 50% and the temperature was maintained at a controlled level of 23° C. Specimens of the S2 form according to ISO 37:2017 were then punched out from these sheets, and the corresponding modulus (stress value of the specimen at 100% elongation according to ISO 37S2) was determined.

[0234] The determined indices are listed in Table 1.

[0235] All samples cured to give tack-free elastomeric materials.

[0236] Table 1:

[0237]

[0238] Surprisingly, the inventive examples 1 to 4 have the desired small reduction in hardness values. This means that the elastomeric properties are maintained under the specified storage conditions.

Claims

1. A composition crosslinkable by condensation reaction, which can be produced using: (A) an organosilicon compound having at least two OH groups, (B) a heterocyclic compound of the formula: A[CR 1 2 SiR a (OR 2 ) 3-a ] x (I), in A represents heterocyclic AH x and contains at least one ring-forming element of the 3rd and / or 5th main groups, in, x hydrogen atoms are bonded to CR 1 2 Replacement of chemical bonds of a group, wherein at least one of these bonds is present on a ring-forming element of the 3rd or 5th main group, R represents identical or different, monovalent, optionally substituted hydrocarbon groups, R 1 may be identical or different and represent a hydrogen atom or a monovalent, optionally substituted hydrocarbon group, R 2 may be the same or different and represent a monovalent, optionally substituted hydrocarbyl group, a = 0 or 1, and x = 1, 2 or 3, and / or its partial hydrolysate as well as (C) at least one compound containing units of the formula: Si(OR 4 ) 3 O 1 / 2 (III), Si(OR 4 ) 2 O 2 / 2 (IV), (OR 4 )SiO 3 / 2 (V) and Optionally SiO 4 / 2 (VI), in R 4 may be the same or different and are independently in each case an alkyl group, Provided that compound (C) contains at least 10 mol % of units of formula (V).

2. The composition according to claim 1, It is characterized in that The organosilicon compounds (A) are those containing units of the formula: R 3 b (OH) c SiO (4-b-c) / 2 (II) in R 3 may be identical or different and represent an optionally substituted hydrocarbyl group which may be interrupted by an oxygen atom, b is 0, 1, 2, or 3, and c is 0, 1, 2, or 3, The conditions are that the sum of b+c is ≤3 and that at least two condensable OH groups are present per molecule.

3. The composition according to claim 1 or 2, It is characterized in that Compound (C) contains units of the formulae (III), (IV) and (V) in a total amount of at least 70 mol %.

4. A composition according to one or more of claims 1 to 3, It is characterized in that Compound (C) contains 10 to 50 mol% of a unit of formula (V), 15 to 60 mol% of a unit of formula (III) and 20 to 60 mol% of a unit of formula (IV).

5. The composition according to one or more of claims 1 to 4, It is characterized in that Compound (C) consists of units of formula (III), (IV), (V) and optionally formula (VI).

6. A composition according to one or more of claims 1 to 5, It is characterized in that The composition includes component (C) in an amount of 1 to 20 parts by weight based on 100 parts by weight of component (A).

7. A composition according to one or more of claims 1 to 6, It is characterized in that The composition is one that can be produced using: (A) an organosilicon compound containing a unit of formula (II), (B) a compound of formula (I), (C) a compound containing units of formula (III), (IV) and (V) in a total amount of at least 80 mol %, provided that the compound contains at least 10 mol % of units of formula (V), optionally, (D) a catalyst, Optionally, (E) a basic nitrogen-containing compound, Optionally, (F) filler, Optionally, (G) an adhesion promoter, Optionally, (H) a plasticizer, Optionally, (J) an additional cross-linking agent, Optionally, (K) additives, and Optionally, (L) a solvent.

8. A composition according to one or more of claims 1 to 7, It is characterized in that The catalyst (D) includes alkoxides of metals of the fourth transition group of the periodic table, carboxylates of metals of the twelfth transition group of the periodic table, and phosphonates.

9. A process for producing a composition as claimed in one or more of claims 1 to 8 by mixing the individual components in any order. 10 . A shaped body produced by crosslinking a composition as claimed in one or more of claims 1 to 8 or by a process as claimed in claim 9 .