Two-component polyurethane adhesive
Through the two-component thermally conductive polyurethane adhesive formulation, the use of polyols, polyisocyanates and aminosilanes, combined with aluminum hydroxide and melamine polyphosphate, the existing adhesives have slow curing speed and high brittleness in aluminum alloy bonding. The problem of impatience achieves high strength and fireproof bonding effect, and is suitable for battery pack applications of electric vehicle battery packs.
Patent Information
- Application Number
- CN202280092771.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-25
- Publication Date
- 2024-11-15
AI Technical Summary
The existing adhesives have problems such as slow curing speed, high brittleness, durability and fire-proofing in the bonding of aluminum alloys and battery components. Especially in harsh climate conditions, the adhesion is significantly reduced, making it difficult to meet the battery packs of electric vehicles. need.
Using a two-component thermally conductive polyurethane adhesive formulation, containing polyhydric alcohols, polyisocyanates and aminosilanes, part A and B are mixed with less than 5 microns of aluminum hydroxide and melamine polyphosphate, forming a high concentration The adhesive provides overlap shear strength of 8MPa or above and flame retardancy at V0 level.
It provides overlap shear strength above 8MPa on aluminum substrate, maintains good adhesion performance under harsh conditions, has V0-level flame retardancy, and meets the structural bonding needs of the battery pack.
Smart Images

Figure BDA0005014983120000051 
Figure BDA0005014983120000151 
Figure BDA0005014983120000221
Abstract
Description
Technical Field
[0001] The present invention relates to the field of adhesives, in particular two-component polyurethane adhesives. Background Art
[0002] Due to the constant pursuit of weight reduction, aluminum alloys are increasingly used in building elements of vehicle body design. Especially for electric vehicles (EV), where the battery brings additional weight to the entire vehicle. The battery itself uses a large amount of aluminum alloys in various structures and components. For example, the housing of the battery pack is usually made of aluminum, and the side panels and edge panels of the battery module are also made of aluminum alloys. The bonding of aluminum alloys to other components of the battery becomes crucial. Adhesive bonding is a currently popular bonding method for aluminum in the automotive industry, which is used together with other bonding methods such as welding and riveting. The typical bonding strength required for bonding structural components should be higher than 5MPa, or preferably higher than 10MPa.
[0003] The most commonly used adhesives for bonding aluminum alloys are based on epoxy and acrylic chemistries. However, epoxy adhesives have relatively slow cure speeds, and they can be brittle in the cured state. This has hampered the use of epoxy adhesives for structural bonding of aluminum alloys inside battery pack applications. Acrylic-based adhesives often have an unpleasant odor, making them less user-friendly.
[0004] Polyurethane (PU) adhesives are commonly used to bond painted substrates and plastic parts in automotive applications. However, PU adhesives generally do not provide a strong, durable bond with aluminum alloys, and in particular, their adhesion to aluminum is significantly reduced when exposed to harsh weather conditions (such as high temperature and high humidity). In addition, for battery applications, the adhesives used inside the battery pack should be fireproof or flame retardant. The flame retardant additives commonly used in the polyurethane industry are halogen-containing or phosphorus-based. Unfortunately, these additives often cause the adhesion or bonding properties of the adhesive to drop sharply, thereby reducing the structural properties of the bonding system. Summary of the invention
[0005] In a first aspect, the present invention provides a two-component thermally conductive polyurethane adhesive formulation comprising:
[0006] (A) Part I, which contains:
[0007] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0008] (B) a second part, which contains:
[0009] (b1) one or more polyether polyols;
[0010] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0011] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture (preferably in a 1:1 volume ratio), the aluminum hydroxide concentration is at least 20 wt% and the melamine polyphosphate concentration is at least 7 wt%.
[0012] A method for bonding two or more substrates, the method comprising the steps of:
[0013] (1) A two-component thermally conductive polyurethane adhesive formulation is provided, comprising:
[0014] (A) Part I, which contains:
[0015] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0016] (B) a second part, which contains:
[0017] (b1) one or more polyether polyols;
[0018] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0019] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %;
[0020] (2) mixing Part A and Part B to provide an uncured adhesive;
[0021] (3) applying the uncured adhesive to at least one substrate;
[0022] (4) placing the uncured adhesive in bonding contact with a second substrate;
[0023] (5) Curing the uncured adhesive.
[0024] An adhesive assembly comprising:
[0025] (1) a first substrate;
[0026] (2) a second substrate;
[0027] wherein the first substrate and the second substrate are adhered to each other by a cured adhesive produced by mixing the following parts A and B together and curing the mixture:
[0028] (A) Part I, which contains:
[0029] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0030] (B) a second part, which contains:
[0031] (b1) one or more polyether polyols;
[0032] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0033] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %. DETAILED DESCRIPTION
[0034] The inventors have discovered that flame retardant adhesives can be formulated with polyurethane to provide i) lap shear strength on aluminum of >8 MPa, ii) a flame retardancy rating of VO, and iii) good retention of lap shear strength after prolonged exposure to harsh conditions.
[0035] Definitions and Abbreviations
[0036] DSC Differential Scanning Calorimetry
[0037] MDI 4,4'-methylenebis(phenyl isocyanate)
[0038] HDI Hexamethylene diisocyanate
[0039] IPDI Isophorone diisocyanate
[0040] PU Polyurethane
[0041] SEC Size Exclusion Chromatography
[0042] RH Relative humidity
[0043] ATH Aluminum Trihydroxide
[0044] MPP Melamine Polyphosphate
[0045] Equivalent weight and molecular weight were measured by gel permeation chromatography (GPC) using a Malvern Viscothek GPC max device. Tetrahydrofuran (THF) was used as eluent, PL GEL MIXED D (Agilent, 300*7.5 mm, 5 μm) was used as a chromatographic column, and MALVERN Viscotek TDA (integrated refractive index viscometer and light scattering) was used as a detector.
[0046] The adhesive of the present invention is a two-component polyurethane adhesive comprising Part A and Part B. Part A and Part B can be packaged together into a kit. Part A and Part B are mixed together in an appropriate ratio (preferably 1:1 by volume) before use, and then applied to one or more substrates as quickly as possible.
[0047] Part A and Part B will now be disclosed in more particular detail.
[0048] Part A (isocyanate)
[0049] Part A comprises a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate, and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties.
[0050] The polyisocyanates used to prepare the prepolymer can be aliphatic, aromatic or a mixture, wherein aromatic polyisocyanates are preferred. Examples of aromatic polyisocyanates include methylene diphenyl diisocyanate (MDI), polycarbodiimide-modified MDI, toluene diisocyanate (TDI), p-phenylene diisocyanate (PPDI) and naphthalene diisocyanate (NDI). MDI and / or polycarbodiimide-modified MDI are particularly preferred. In certain embodiments, a mixture of MDI and polycarbodiimide-modified MDI is used.
[0051] The polyisocyanate used for preparing the prepolymer is preferably used in an amount of 35 to 65 wt %, based on the total weight of component A, more preferably 40 to 60 wt %, particularly preferably 45 to 55 wt %.
[0052] In a particularly preferred embodiment, the prepolymer is prepared using 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, based on the total weight of component A, of MDI and / or polycarbodiimide-modified MDI.
[0053] The polyol used to prepare the prepolymer is preferably a polyether polyol. The polyol may have two or more OH groups. Examples of polyether polyols include poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, particularly preferably the alkylene group is C2-C4. Examples of suitable polyols include poly(ethylene oxide) polyols, poly(propylene oxide) polyols, poly(tetrahydrofuran) polyols. Particularly preferred are poly(propylene oxide) polyols, in particular poly(propylene glycol). In a preferred embodiment, the polyether polyol is a polyether polyol based on propylene glycol. In a particularly preferred embodiment, it is a polyether polyol based on propylene glycol with ethylene oxide termination, having a molecular weight of about 2,000 Da and a functionality of 2.
[0054] The polyether polyols used for preparing the prepolymers are preferably used in an amount of 5 to 20 wt %, based on the total weight of component A, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %.
[0055] In a preferred embodiment, the polyol used to prepare the prepolymer is a propylene glycol-based polyether polyol, which is used in an amount of 5 to 20 wt %, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %, based on the total weight of component A.
[0056] The polyisocyanate is used in excess of the polyether polyol so that the prepolymer is terminated with isocyanate groups.The final prepolymer preferably has an NCO wt% in the range of 5-30 wt%, more preferably in the range of 10-25 wt%.
[0057] The aminosilane in component A preferably has the general formula I or the general formula II:
[0058]
[0059] Where R 1 are independently selected from C1-C6 alkyl, and R 2 Independently selected from C2-C6 alkylene.
[0060] In a preferred embodiment, the aminosilane in component A has the general formula I, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group. In a more preferred embodiment, the aminosilane has the general formula I, R 1 is methyl, and R2 is propylene.
[0061] In another preferred embodiment, the aminosilane in component A has the general formula II, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group. In a more preferred embodiment, the aminosilane has the general formula II, R 1 is methyl, and R2 is propylene.
[0062] In a particularly preferred embodiment, the aminosilane in component A is bis-(trimethoxysilylpropyl)amine.
[0063] The aminosilane in component A is preferably used in an amount of 0.5 to 4 wt %, based on the total weight of component A, more preferably 1 to 3 wt %, particularly preferably 1.5 to 2.5 wt %.
[0064] In a preferred embodiment, the aminosilane in component A is bis-(trimethoxysilylpropyl)amine, which is used in an amount of 0.5-4 wt %, more preferably 1-3 wt %, and particularly preferably 1.5-2.5 wt %, based on the total weight of component A.
[0065] In a preferred embodiment, the prepolymer in component A is prepared using:
[0066] 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, of polyisocyanate, based on the total weight of component A;
[0067] 5-20 wt %, more preferably 8-15 wt %, particularly preferably 9-12 wt %, of polyether polyol, based on the total weight of component A; and
[0068] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of aminosilane.
[0069] In a more preferred embodiment, the prepolymer in component A is prepared using:
[0070] 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, based on the total weight of component A, of MDI and / or polycarbodiimide-modified MDI, or a mixture of MDI and polycarbodiimide-modified MDI;
[0071] 5 to 20 wt %, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol, preferably based on a polyether polyol having an OH number (mg KOH / g) of 109-115; and
[0072] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of an aminosilane having the general formula II, wherein R 1 is C1-C2 alkyl, and R2 is C2-C4 alkylene, more preferably R 1 is methyl, and R2 is propylene.
[0073] In a particularly preferred embodiment, the prepolymer in component A is prepared using:
[0074] 45-55 wt% of a mixture of MDI and polycarbodiimide-modified MDI, based on the total weight of component A;
[0075] 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol having an OH number (mg KOH / g) of 109-115; and
[0076] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of bis-(trimethoxysilylpropyl)amine.
[0077] The prepolymer is prepared by mixing the components, preferably under dry and / or inert atmosphere, for a period of time sufficient to cause substantially all of the OH groups of the polyol and the amino groups of the aminosilane to react with the polyisocyanate. In a preferred embodiment, the mixing is carried out for 1 to 2 hours. The ratio is selected so that the prepolymer is terminated with isocyanate groups and part of the silane groups.
[0078] Part B (polyols)
[0079] Part B contains:
[0080] one or more polyether polyols; and
[0081] One or more catalysts capable of promoting the reaction of the NCO portion of the prepolymer with the polyol of component B.
[0082] The polyol used in component B is a polyether polyol. The polyol may have two or more OH groups. Examples of polyether polyols include poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, particularly preferably the alkylene group is C2-C4. Examples of suitable polyols include poly(ethylene oxide) polyols, poly(propylene oxide) polyols, poly(tetramethylene oxide) polyols. Particularly preferred are poly(propylene oxide) polyols.
[0083] In a preferred embodiment, the polyether polyol of component B is a mixture of polyols having a functionality of 2 to 6. In a particularly preferred embodiment, the polyether polyol of component B is a mixture of at least one diol, at least one triol and at least one polyol with a functionality>3.
[0084] In a preferred embodiment, the polyether polyol of component B is a mixture comprising or consisting of a diol, a triol, and a polyol having a nominal functionality of 5-6.
[0085] In a preferred embodiment, the polyether polyol of component B is a mixture of poly(propylene oxide) polyols having a functionality of 2 to 6. In a particularly preferred embodiment, the polyether polyol of component B is a mixture comprising or consisting of at least one poly(propylene oxide) diol, at least one poly(propylene oxide) triol and at least one poly(propylene oxide) polyol having a functionality > 3.
[0086] In a preferred embodiment, the polyether polyol of component B is a mixture comprising or consisting of poly(propylene oxide) diol, poly(propylene oxide) triol and poly(propylene oxide) polyol having a nominal functionality of 5-6.
[0087] In another preferred embodiment, the polyether polyol of component B comprises, based on the total weight of the polyether polyols in component B, 46-83 wt % of polyether triol, 19-46 wt % of polyether polyol with functionality>3, and 4-15 wt % of polyether diol.
[0088] In another preferred embodiment, the polyether polyol of component B comprises, based on the total weight of the polyether polyols in component B, 55-65 wt% of polyether triol, 25-35 wt% of polyether polyol with functionality>3, and 5-8 wt% of polyether diol.
[0089] In another preferred embodiment, the polyether polyol of component B comprises 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with a functionality > 3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
[0090] In another preferred embodiment, the polyether polyol of component B comprises 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with a functionality > 3, and 5-8 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
[0091] The total polyether polyol in component B is preferably present in an amount of 35 to 70 wt %, based on the total weight of component B, more preferably 40 to 60 wt %, particularly preferably 50 to 57 wt %.
[0092] In a preferred embodiment, component B comprises 35 to 70 wt %, more preferably 40 to 60 wt %, particularly preferably 50 to 57 wt %, based on the total weight of component B, of a mixture of polyether polyols, the mixture comprising or consisting of:
[0093] (1) based on the total weight of the polyether polyol in component B, 46-83 wt% of polyether triol, 19-46 wt% of polyether polyol with a functionality > 3, and 4-15 wt% of polyether diol; or
[0094] (2) based on the total weight of the polyether polyol in component B, 55-65 wt% of a polyether triol, 25-35 wt% of a polyether polyol having a functionality > 3, and 5-8 wt% of a polyether diol; or
[0095] (3) 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with functionality>3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B; or
[0096] (4) Based on the total weight of the polyether polyol in component B, 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with a functionality > 3, and 5-8 wt% of poly(propylene oxide) diol.
[0097] Component B may optionally comprise a diol having a molecular weight <200 Da, more preferably <150 Da. Examples include propylene glycol and butanediol, with butanediol (eg 1,4-butanediol) being particularly preferred.
[0098] If present, diols with a molecular weight <200 Da are preferably used in an amount of 5 to 12 wt %, based on the total weight of component B, more preferably 6-10 wt %, particularly preferably 8-9 wt %.
[0099] In a preferred embodiment, component B contains 5 to 12 wt %, more preferably 6-10 wt %, particularly preferably 8-9 wt %, of butanediol (eg 1,4-butanediol), based on the total weight of component B.
[0100] Component B comprises one or more catalysts capable of promoting the reaction of the NCO moieties of the prepolymer of Component A with the one or more polyether polyols of Component B.
[0101] The catalyst is preferably selected from Lewis bases and Lewis acids. Preferred are tertiary amines, including diazabicyclo[2.2.2]octane, tri-2,4,6-((dimethylamino)methyl)phenol, DMDEE (2,2'-dimorpholine diethyl ether), imidazole (such as 4-methylimidazole), triethanolamine, polyethyleneimine, among which diazabicyclo[2.2.2]octane is particularly preferred.
[0102] Also suitable are organotin compounds such as dioctyl dineodecanoyl oxide, dibutyltin di(acetate), and di-n-octyltin bis(isooctyl mercaptoacetate), of which dibutyltin di(acetate) is particularly preferred.
[0103] In a preferred embodiment, the catalyst comprises diazabicyclo[2.2.2]octane and dibutyltin di(acetate).
[0104] The catalyst is preferably used in an amount of 0.05 to 0.5 wt %, based on the total weight of component B, more preferably 0.1 to 0.3 wt %, particularly preferably 0.2 wt %.
[0105] In a preferred embodiment, the catalyst is a mixture of diazabicyclo[2.2.2]octane and dibutyltin diacetate, which is used in an amount of 0.05-0.5 wt %, more preferably 0.1-0.3 wt %, particularly preferably 0.2 wt %, based on the total weight of component B.
[0106] Aluminum hydroxide and melamine polyphosphate
[0107] Part A and / or part B contain D having less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture (preferably in a 1:1 volume ratio), the aluminum hydroxide concentration is at least 20 wt%, and the melamine polyphosphate concentration is at least 7 wt%, both based on the total weight of the mixture. Particle size and distribution are measured by light scattering using acetone as the suspension medium.
[0108] Preferably, the concentration of aluminum hydroxide in the binder mixture is 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture.
[0109] In a preferred embodiment, aluminum hydroxide is present in component A at 20-35 wt %, more preferably 22-26 wt %, based on the total weight of component A.
[0110] In another preferred embodiment, aluminum hydroxide is present in component B at 20-35 wt %, more preferably 22-26 wt %, based on the total weight of component B.
[0111] In a preferred embodiment, aluminum hydroxide is present in both component A and component B.
[0112] In another preferred embodiment, aluminum hydroxide is present in both component A and component B at 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components.
[0113] In a preferred embodiment, the aluminum hydroxide has a D of less than 3 microns, more preferably about 1 micron. 50 .
[0114] Preferably, the adhesive mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) contains 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0115] In a preferred embodiment, component A comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component A, of a D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0116] In another preferred embodiment, component B comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component B, of a D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0117] In another preferred embodiment, both component A and component B contain 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0118] Preferably, the concentration of melamine polyphosphate in the adhesive mixture is 7-15 wt %, more preferably 8-12 wt %, particularly preferably 9-11 wt %, based on the total weight of the mixture.
[0119] In a preferred embodiment, melamine polyphosphate is present in component A at 7-15 wt %, more preferably 8-12 wt %, based on the total weight of component A.
[0120] In another preferred embodiment, melamine polyphosphate is present in component B at 7-15 wt %, more preferably 8-12 wt %, based on the total weight of component B.
[0121] In a preferred embodiment, melamine polyphosphate is present in both component A and component B.
[0122] In another preferred embodiment, melamine polyphosphate is present in both component A and component B at 7-15 wt%, more preferably 8-12 wt%, based on the total weight of the respective components.
[0123] Optional ingredients in components A and B
[0124] Components A and / or B may additionally contain other ingredients, for example talc, molecular sieves, silicon dioxide (especially amorphous silicon dioxide), carbon black.
[0125] Apply to substrate
[0126] Part (A) and part (B) are mixed and can be applied to the substrate using known methods such as a manual application system or in an automatic manner with a pump system using a 20 1 pail or a 200 1 drum or any other preferred container.
[0127] Preferred substrates include aluminum, e-coated aluminum, e-coated steel, laser treated aluminum, or passivated aluminum.
[0128] Characterization
[0129] When measured according to the method given in the examples, the cured adhesive composition obtained by mixing components A and B, after being cured at 23° C., 50% relative humidity and left to stand for 7 days, has an overlap shear strength on an aluminum substrate of preferably 8 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
[0130] When measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B is cured at 23°C, 50% relative humidity and left to stand for 7 days, followed by 7 days of Cataplasma treatment, and the lap shear strength on the aluminum substrate is preferably 6 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
[0131] When measured according to the method given in the examples, the lap shear strength of the cured adhesive composition obtained by mixing components A and B, after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and then cured at 85°C and 85% relative humidity and left to stand for 168 hours, on an aluminum substrate is preferably 8 MPa or more, more preferably 10 MPa or more, and particularly preferably 11 MPa or more.
[0132] When measured according to the method given in the examples, the lap shear strength on an aluminum substrate of the cured adhesive composition obtained by mixing components A and B, after being cured at 23° C., 50% relative humidity and left to stand for 7 days, and then cured at 85° C. and 85% relative humidity and left to stand for 1,000 hours, is preferably 8 MPa or more, more preferably 10 MPa or more, and particularly preferably 11 MPa or more.
[0133] The cured adhesive composition obtained by mixing components A and B preferably has a UL94 rating of V0 after curing for 7 days at 23° C. and 50% relative humidity.
[0134] In a preferred embodiment, when measured according to the method given in the examples, the cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength on an aluminum substrate of 8 MPa or more, more preferably 9 MPa or more, particularly preferably 10 MPa or more, after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and has a UL94 rating of V0 after being cured at 23°C and 50% relative humidity for 7 days.
[0135] In another preferred embodiment, the cured adhesive (7 days at 23°C and 50% relative humidity) has a lap shear strength of 6 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater on an aluminum substrate after 7 days of poultice treatment when measured according to the method given in the examples, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
[0136] In another preferred embodiment, when measured according to the method given in the examples, the cured adhesive (7 days at 23°C and 50% relative humidity) has a lap shear strength on an aluminum substrate of 8 MPa or more, more preferably 10 MPa or more, particularly preferably 11 MPa or more, after 168 hours at 85°C and 85% relative humidity, and has a UL94 rating of V0 after curing for 7 days at 23°C and 50% relative humidity.
[0137] In another preferred embodiment, when measured according to the method given in the examples, the cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength on an aluminum substrate of 8 MPa or more, more preferably 10 MPa or more, particularly preferably 11 MPa or more, after 1,000 hours at 85°C and 85% relative humidity, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
[0138] Particularly preferred embodiments
[0139] The following are particularly preferred embodiments of the present invention:
[0140] 1. A two-component thermally conductive polyurethane adhesive formulation comprising:
[0141] (A) Part I, which contains:
[0142] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0143] (B) a second part, which contains:
[0144] (b1) one or more polyether polyols;
[0145] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0146] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %.
[0147] 2. A method for bonding two or more substrates, the method comprising the steps of:
[0148] (1) A two-component thermally conductive polyurethane adhesive formulation is provided, comprising:
[0149] (A) Part I, which contains:
[0150] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0151] (B) a second part, which contains:
[0152] (b1) one or more polyether polyols;
[0153] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0154] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %;
[0155] (2) mixing Part A and Part B to provide an uncured adhesive;
[0156] (3) applying the uncured adhesive to at least one substrate;
[0157] (4) placing the uncured adhesive in bonding contact with a second substrate;
[0158] (5) Curing the uncured adhesive.
[0159] 3. An adhesive assembly comprising:
[0160] (1) a first substrate;
[0161] (2) a second substrate;
[0162] wherein the first substrate and the second substrate are adhered to each other by a cured adhesive produced by mixing the following parts A and B together and curing the mixture:
[0163] (A) Part I, which contains:
[0164] (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties;
[0165] (B) a second part, which contains:
[0166] (b1) one or more polyether polyols;
[0167] (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1);
[0168] Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %.
[0169] 4. As described in any preceding embodiment, wherein the polyisocyanate used to prepare the prepolymer is aromatic.
[0170] 5. As described in any of the preceding embodiments, the polyisocyanate used to prepare the prepolymer is selected from methylene diphenyl diisocyanate (MDI), polycarbodiimide-modified MDI, toluene diisocyanate (TDI), p-phenylene diisocyanate (PPDI), naphthalene diisocyanate (NDI), and mixtures thereof.
[0171] 6. As described in any preceding embodiment, the polyisocyanate used to prepare the prepolymer is selected from MDI, polycarbodiimide-modified MDI, and mixtures thereof.
[0172] 7. As described in any of the preceding embodiments, the polyisocyanate used to prepare the prepolymer is used in an amount of 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, based on the total weight of component A.
[0173] 8. As described in any of the preceding embodiments, wherein the prepolymer is prepared using 35-65 wt%, more preferably 40-60 wt%, particularly preferably 45-55 wt% of MDI and / or polycarbodiimide-modified MDI based on the total weight of component A.
[0174] 9. As described in any preceding embodiment, wherein the polyol used to prepare the prepolymer is a polyether polyol.
[0175] 10. As described in any preceding embodiment, wherein the polyol used to prepare the prepolymer has two or more OH groups.
[0176] 11. As described in any of the preceding embodiments, the polyol used to prepare the prepolymer is selected from poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, particularly preferably the alkylene group is C2-C4.
[0177] 12. As described in any preceding embodiment, wherein the polyol used to prepare the prepolymer is a poly(propylene oxide) polyol.
[0178] 13. As described in any preceding embodiment, wherein the polyol used to prepare the prepolymer is a propylene glycol-based polyether polyol with ethylene oxide end-capping, the polyether polyol having a molecular weight of about 2,000 Da and a functionality of 2.
[0179] 14. As described in any of the preceding embodiments, wherein the polyol used to prepare the prepolymer is used in an amount of 5 to 20 wt %, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %, based on the total weight of component A.
[0180] 15. As described in any of the preceding embodiments, the polyol used to prepare the prepolymer is a propylene glycol-based polyether polyol, which is used in an amount of 5 to 20 wt%, more preferably 8 to 15 wt%, and particularly preferably 9 to 12 wt%, based on the total weight of component A.
[0181] 16. As described in any preceding embodiment, wherein the polyisocyanate is used in an amount in excess of the polyether polyol such that the prepolymer is terminated with isocyanate groups.
[0182] 17. As in any preceding embodiment, wherein the prepolymer is terminated with isocyanate groups, wherein the NCO wt% is in the range of 5% to 30%, preferably in the range of 10% to 25%.
[0183] 18. As described in any of the preceding embodiments, wherein the aminosilane in component A preferably has the general formula I or the general formula II:
[0184]
[0185] Where R 1 are independently selected from C1-C6 alkyl, and R 2 Independently selected from C2-C6 alkylene.
[0186] 19. As described in Example 18, wherein the aminosilane in component A has the general formula I, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group.
[0187] 20. As described in embodiment 18, wherein the aminosilane has the general formula I, R 1 is methyl, and R2 is propylene.
[0188] 21. As described in Example 18, wherein the aminosilane in component A has the general formula II, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group.
[0189] 22. As described in embodiment 18, wherein the aminosilane has the general formula II, R 1 is methyl, and R2 is propylene.
[0190] 23. As described in any preceding embodiment, wherein the aminosilane in component A is bis-(trimethoxysilylpropyl)amine.
[0191] 24. As described in any of the preceding embodiments, wherein the aminosilane in component A is used in an amount of 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A.
[0192] 25. As described in any of the preceding embodiments, wherein the aminosilane in component A is bis-(trimethoxysilylpropyl)amine, and the bis-(trimethoxysilylpropyl)amine is used in an amount of 0.5-4 wt%, more preferably 1-3 wt%, and particularly preferably 1.5-2.5 wt%, based on the total weight of component A.
[0193] 26. As described in any of the preceding embodiments, wherein the prepolymer in component A is prepared using:
[0194] 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, of polyisocyanate, based on the total weight of component A;
[0195] 5-20 wt %, more preferably 8-15 wt %, particularly preferably 9-12 wt %, of polyether polyol, based on the total weight of component A; and
[0196] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of aminosilane.
[0197] 27. As described in any of the preceding embodiments, wherein the prepolymer in component A is prepared using:
[0198] 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, based on the total weight of component A, of MDI and / or polycarbodiimide-modified MDI, or a mixture of MDI and polycarbodiimide-modified MDI;
[0199] 5 to 20 wt %, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol, preferably based on a polyether polyol having an OH number (mg KOH / g) of 109-115; and
[0200] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of an aminosilane having the general formula II, wherein R 1 is C1-C2 alkyl, and R2 is C2-C4 alkylene, more preferably R 1 is methyl, and R2 is propylene.
[0201] 28. As described in any of the preceding embodiments, wherein the prepolymer in component A is prepared using:
[0202] 45-55 wt% of a mixture of MDI and polycarbodiimide-modified MDI, based on the total weight of component A;
[0203] 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol having an OH number (mg KOH / g) of 109-115; and
[0204] 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of bis-(trimethoxysilylpropyl)amine.
[0205] 29. As described in any of the preceding embodiments, the polyether polyol used in component B is selected from poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, particularly preferably the alkylene group is C2-C4, and mixtures of these.
[0206] 30. As described in any preceding embodiment, wherein the polyether polyol used in component B is selected from poly(propylene oxide) polyols, and mixtures of these.
[0207] 31. As described in any preceding embodiment, wherein the polyether polyol used in component B is a mixture of polyols having a functionality of 2-6.
[0208] 32. As described in any preceding embodiment, wherein the polyether polyol used in component B is a mixture of at least one diol, at least one triol and at least one polyol with a functionality >3.
[0209] 33. As described in any preceding embodiment, wherein the polyether polyol used in Component B is a mixture comprising or consisting of a diol, a triol, and a polyol having a nominal functionality of 5-6.
[0210] 34. As described in any preceding embodiment, wherein the polyether polyol used in Component B is a mixture of poly(propylene oxide) polyols having a functionality of 2-6.
[0211] 35. As described in any preceding embodiment, the polyether polyol used in component B is a mixture comprising or consisting of at least one poly(propylene oxide) diol, at least one poly(propylene oxide) triol and at least one poly(propylene oxide) polyol with a functionality >3.
[0212] 36. As described in any preceding embodiment, the polyether polyol used in component B is a mixture comprising or consisting of a poly(propylene oxide) diol, a poly(propylene oxide) triol, and a poly(propylene oxide) polyol having a nominal functionality of 5-6.
[0213] 37. As described in any of the preceding embodiments, the polyether polyol used in component B comprises 46-83 wt% of polyether triol, 19-46 wt% of polyether polyol with a functionality > 3, and 4-15 wt% of polyether diol, based on the total weight of the polyether polyol in component B.
[0214] 38. As described in any of the preceding embodiments, the polyether polyol used in component B comprises 55-65 wt% of polyether triol, 25-35 wt% of polyether polyol with a functionality > 3, and 5-8 wt% of polyether diol, based on the total weight of the polyether polyol in component B.
[0215] 39. As described in any of the preceding embodiments, the polyether polyol used in component B comprises 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with a functionality > 3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
[0216] 40. As described in any of the preceding embodiments, the polyether polyol used in component B comprises 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with a functionality > 3, and 5-8 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
[0217] 41. As described in any of the preceding embodiments, the polyether polyol used in component B is used in an amount of 35 to 70 wt %, more preferably 40 to 60 wt %, particularly preferably 50 to 57 wt %, based on the total weight of component B.
[0218] 42. As described in any of the preceding embodiments, component B comprises 35 to 70 wt%, more preferably 40 to 60 wt%, particularly preferably 50 to 57 wt%, based on the total weight of component B, of a mixture of polyether polyols, the mixture comprising or consisting of:
[0219] (1) based on the total weight of the polyether polyol in component B, 46-83 wt% of polyether triol, 19-46 wt% of polyether polyol with a functionality > 3, and 4-15 wt% of polyether diol; or
[0220] (2) based on the total weight of the polyether polyol in component B, 55-65 wt% of a polyether triol, 25-35 wt% of a polyether polyol having a functionality > 3, and 5-8 wt% of a polyether diol; or
[0221] (3) 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with functionality>3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B; or
[0222] (4) Based on the total weight of the polyether polyol in component B, 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with a functionality > 3, and 5-8 wt% of poly(propylene oxide) diol.
[0223] 43. As described in any preceding embodiment, wherein component B comprises a diol with a molecular weight of <200 Da, more preferably <150 Da.
[0224] 44. As described in any preceding embodiment, wherein component B comprises a diol selected from propylene glycol, butylene glycol, and mixtures thereof.
[0225] 45. As described in any preceding embodiment, wherein component B comprises butanediol (eg, 1,4-butanediol), which is particularly preferred.
[0226] 46. As described in any of the preceding embodiments, wherein component B comprises 5 to 12 wt%, more preferably 6-10 wt%, particularly preferably 8-9 wt%, based on the total weight of component B, of a diol having a molecular weight <200 Da.
[0227] 47. As described in any of the preceding embodiments, wherein component B comprises 5 to 12 wt %, more preferably 6-10 wt %, and particularly preferably 8-9 wt % of butanediol (eg, 1,4-butanediol), based on the total weight of component B.
[0228] 48. As described in any preceding embodiment, wherein the catalyst is selected from Lewis bases and Lewis acids.
[0229] 49. As described in any preceding embodiment, the catalyst comprises a catalyst selected from diazabicyclo[2.2.2]octane, tris-2,4,6-((dimethylamino)methyl)phenol, DMDEE (2,2'-dimorpholinodiethyl ether), imidazole (such as 4-methylimidazole), triethanolamine, polyethyleneimine, and mixtures of these.
[0230] 50. As described in any preceding embodiment, wherein the catalyst comprises diazabicyclo[2.2.2]octane.
[0231] 51. As described in any preceding embodiment, wherein the catalyst comprises an organotin compound.
[0232] 52. As described in any preceding embodiment, the catalyst comprises an organotin compound selected from dioctyl dineodecanoyl oxide, dibutyltin di(acetate), and di-n-octyltin bis(isooctyl thioglycolate), and mixtures thereof.
[0233] 53. As described in any preceding embodiment, wherein the catalyst comprises dibutyltin di(acetate).
[0234] 54. As described in any preceding embodiment, the catalyst comprises diazabicyclo[2.2.2]octane and dibutyltin di(acetate).
[0235] 55. As described in any of the preceding embodiments, wherein the catalyst is used in an amount of 0.05-0.5 wt%, more preferably 0.1-0.3 wt%, particularly preferably 0.2 wt%, based on the total weight of component B.
[0236] 56. As described in any of the preceding embodiments, wherein the catalyst is a mixture of diazabicyclo[2.2.2]octane and dibutyltin diacetate, the mixture being used in an amount of 0.05-0.5 wt%, more preferably 0.1-0.3 wt%, particularly preferably 0.2 wt%, based on the total weight of component B.
[0237] 57. As described in any preceding embodiment, the concentration of aluminum hydroxide in the binder mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) is 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture.
[0238] 58. As described in any of the preceding embodiments, the aluminum hydroxide is present in component A at 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component A.
[0239] 59. As described in any of the preceding embodiments, the aluminum hydroxide is present in component B at 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component B.
[0240] 60. As described in any preceding embodiment, wherein the aluminum hydroxide is present in both component A and component B.
[0241] 61. As described in any preceding embodiment, the aluminum hydroxide is present in both component A and component B at 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components.
[0242] 62. As described in any of the preceding embodiments, wherein the aluminum hydroxide has a D of less than 3 microns, more preferably about 1 micron. 50 .
[0243] 63. As described in any of the preceding embodiments, the adhesive mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0244] 64. As described in any of the preceding embodiments, wherein component A comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component A, of a D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0245] 65. As described in any of the preceding embodiments, wherein component B comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component B, of a D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0246] 66. As described in any of the preceding embodiments, wherein both component A and component B contain 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
[0247] 67. As described in any of the preceding embodiments, the concentration of melamine polyphosphate in the adhesive mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) is 7-15 wt%, more preferably 8-12 wt%, and particularly preferably 9-11 wt%, based on the total weight of the mixture.
[0248] 68. As described in any preceding embodiment, wherein the melamine polyphosphate is present in component A at 7-15 wt %, more preferably 8-12 wt %, based on the total weight of component A.
[0249] 69. As described in any preceding embodiment, wherein the melamine polyphosphate is present in component B at 7-15 wt %, more preferably 8-12 wt %, based on the total weight of component B.
[0250] 70. As described in any preceding embodiment, wherein melamine polyphosphate is present in both component A and component B.
[0251] 71. As described in any preceding embodiment, wherein melamine polyphosphate is present in both component A and component B at 7-15 wt%, more preferably 8-12 wt%, based on the total weight of the respective components.
[0252] 72. As described in any of the preceding embodiments, when measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B, after being cured at 23° C., 50% relative humidity and left to stand for 7 days, has a lap shear strength on an aluminum substrate of preferably 8 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
[0253] 73. As described in any of the foregoing embodiments, wherein when measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B is cured at 23°C and 50% relative humidity and left to stand for 7 days, followed by 7 days of poultice treatment, the lap shear strength on the aluminum substrate is preferably 6 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
[0254] 74. As described in any of the preceding embodiments, when measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B is cured at 23°C and 50% relative humidity and allowed to stand for 7 days, and then cured at 85°C and 85% relative humidity and allowed to stand for 168 hours, and the lap shear strength on an aluminum substrate is preferably 8 MPa or greater, more preferably 10 MPa or greater, and particularly preferably 11 MPa or greater.
[0255] 75. As described in any of the preceding embodiments, wherein the lap shear strength on an aluminum substrate of the cured adhesive composition obtained by mixing components A and B, after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and then cured at 85°C and 85% relative humidity and left to stand for 1,000 hours, when measured according to the method given in the example, is preferably 8 MPa or greater, more preferably 10 MPa or greater, and particularly preferably 11 MPa or greater.
[0256] 76. As described in any preceding embodiment, wherein the cured adhesive composition obtained by mixing components A and B preferably has a UL94 rating of V0 after curing for 7 days at 23°C and 50% relative humidity.
[0257] 77. As described in any of the preceding embodiments, when measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength on an aluminum substrate of 8 MPa or greater, more preferably 9 MPa or greater, particularly preferably 10 MPa or greater after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and has a UL94 rating of V0 after being cured at 23°C and 50% relative humidity for 7 days.
[0258] 78. As described in any of the foregoing embodiments, when measured according to the method given in the example, the cured adhesive (7 days at 23°C and 50% relative humidity) has a lap shear strength on an aluminum substrate of 6 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater after 7 days of poultice treatment, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
[0259] 79. As described in any of the preceding embodiments, when measured according to the method given in the example, the cured adhesive (7 days at 23°C and 50% relative humidity) has a lap shear strength on an aluminum substrate of 8 MPa or greater, more preferably 10 MPa or greater, particularly preferably 11 MPa or greater after 168 hours at 85°C and 85% relative humidity, and has a UL94 rating of V0 after curing for 7 days at 23°C and 50% relative humidity.
[0260] 80. As described in any of the preceding embodiments, wherein the cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength of 8 MPa or greater, more preferably 10 MPa or greater, particularly preferably 11 MPa or greater on an aluminum substrate after 1,000 hours at 85°C and 85% relative humidity, when measured according to the method given in the example, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
[0261] Examples
[0262]
[0263]
[0264] Preparation of Part A (isocyanate component)
[0265] First, the MDI, polyether polyol and aminosilane (Dynasilan 1124) in the amounts listed in Table 2 were loaded into a planetary mixer and mixed at a mixing speed between 300-1,000 rpm for 2 hours at room temperature, and then fillers ATH, MPP, talc, carbon black and amorphous silica were loaded into the mixture. These fillers were pre-dried in an oven at a temperature of 100° C.-200° C. until the moisture level was below 1,000 ppm. The fillers were mixed into the mixture at a mixing speed of 1,000-2,000 rpm within 30-60 minutes. The mixture was then loaded into a barrel for storage.
[0266] Production of Part B (Polyol Component)
[0267] The polyol, silane (Dynasilan) and catalyst in the amounts shown in Table 2 were mixed at 500-1,000 rpm for 5-15 minutes, and then fillers ATH, MPP, talc, amorphous silica and molecular sieves were loaded into the mixture. These fillers were pre-dried in an oven at a temperature of 100° C.-200° C. until the moisture level was below 1,000 ppm. The fillers were mixed into the mixture at a mixing speed of 1,000-2,000 rpm within 30-60 minutes. The mixture was then loaded into a barrel for storage.
[0268] Use of adhesives
[0269] Parts A and B are mixed in a 1:1 volume ratio using a static mixer and can be dispensed onto the substrate manually or automatically.
[0270] method
[0271] Flammability
[0272] Adhesive samples were produced by mixing parts A and B in a 1:1 volume ratio and curing the mixture at 23°C at 50% relative humidity for 7 days. The flammability of the samples was measured according to the UL94 flame test. If the burning stopped within 10 seconds on a vertical specimen, the sample was assigned a V0 rating; dripping particles were allowed as long as the particles did not burn. The results are reported in Table 2.
[0273] Lap shear test
[0274] The lap shear strength was measured on aluminum alloy 3003 according to DIN EN1465. An aluminum substrate (from Novelis, AA6061 T6 1.92mm MF noPT no lub, 140x 25mm, 1.9mm thick) was used. The substrate was cleaned with isopropyl alcohol before use. The adhesive was produced by mixing parts A and B in a volume ratio of 1:1 and applied to one substrate, and then the second substrate was joined within 5 minutes. The thickness was adjusted to 1.0mm, and the overlap area was 25mm×25mm. Before the lap shear test, the material was cured and left to stand for 7 days at 23°C and 50% relative humidity. The lap shear sample was then installed in a tensiometer and the lap shear test was performed using a pulling speed of 10mm / min. The force deflection curve was monitored, and the fracture strength was reported as the lap shear strength.
[0275] Lap shear testing was performed immediately after cure, after 7 days of cataplasm exposure (cataplasm conditioning was 7 days at 70°C, 100% relative humidity followed by 24 hours of heat shock at -30°C), after 168 hours at 85°C and 85% relative humidity, and after 1,000 hours at 85°C and 85% relative humidity. The results are reported in Table 2.
[0276]
[0277]
[0278]
[0279] Inventive Examples 1-4 all exhibited a UL94 rating of V0 and exhibited excellent shear strength (≥11 MPa) immediately after curing. Comparative Examples 5, 6, and 9 had unacceptable UL94 ratings and also exhibited lower lap shear strength (<11 MPa) immediately after curing. Comparative Examples 7 and 8 had a rating of V0, however, their lap shear strengths immediately after curing were significantly lower (<9 MPa).
[0280] Inventive Examples 2 and 3 showed excellent retention of lap shear strength after 7 days of cataplasm treatment and after 168 hours at 85°C and 85% relative humidity. In contrast, Comparative Examples 5 and 6 showed an unacceptable decrease in lap shear strength after 7 days of cataplasm treatment, and Comparative Examples 5 and 8 showed an unacceptable decrease in lap shear strength after 168 hours at 85°C and 85% relative humidity.
Claims
1. A two-component thermally conductive polyurethane adhesive formulation comprising: (A) a first part, the first part comprising: (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties; (B) a second part, the second part comprising: (b1) one or more polyether polyols; (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1); Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %.
2. A method for bonding two or more substrates, the method comprising the steps of: (1) A two-component thermally conductive polyurethane adhesive formulation is provided, comprising: (A) a first part, the first part comprising: (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties; (B) a second part, the second part comprising: (b1) one or more polyether polyols; (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1); Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %; (2) mixing Part A and Part B to provide an uncured adhesive; (3) applying the uncured adhesive to at least one substrate; (4) placing the uncured adhesive in bonding contact with a second substrate; (5) Curing the uncured adhesive.
3. An adhesive assembly comprising: (1) a first substrate; (2) a second substrate; wherein the first substrate and the second substrate are adhered to each other by a cured adhesive produced by mixing the following parts A and B together and curing the mixture: (A) a first part, the first part comprising: (a1) a polyurethane prepolymer prepared from at least one polyol, at least one polyisocyanate and an aminosilane, wherein the prepolymer is partially terminated with silane moieties and has reactive NCO moieties; (B) a second part, the second part comprising: (b1) one or more polyether polyols; (b2) one or more catalysts capable of promoting the reaction of the NCO moieties of (a1) with (b1); Wherein part A and / or part B comprises D having a diameter less than 5 microns 50 Aluminum hydroxide, and melamine polyphosphate, such that when Part A and Part B are mixed together to form a binder mixture, the aluminum hydroxide concentration is at least 20 wt % and the melamine polyphosphate concentration is at least 7 wt %.
4. A method as claimed in any preceding claim, wherein: The polyisocyanate used to prepare the prepolymer is aromatic.
5. A method as claimed in any preceding claim, wherein: The polyisocyanate used to prepare the prepolymer is selected from methylene diphenyl diisocyanate (MDI), polycarbodiimide-modified MDI, toluene diisocyanate (TDI), p-phenylene diisocyanate (PPDI), naphthalene diisocyanate (NDI), and mixtures thereof.
6. A method as claimed in any preceding claim, wherein: The polyisocyanate used to prepare the prepolymer is selected from MDI, polycarbodiimide-modified MDI, and mixtures of these.
7. A method as claimed in any preceding claim, wherein: The polyisocyanate used for preparing the prepolymer is used in an amount of 35-65 wt %, based on the total weight of component A, more preferably 40-60 wt %, particularly preferably 45-55 wt %.
8. A method as claimed in any preceding claim, wherein: The prepolymer is prepared using 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, of MDI and / or polycarbodiimide-modified MDI, based on the total weight of component A.
9. A method as claimed in any preceding claim, wherein: The polyol used to prepare the prepolymer is a polyether polyol.
10. A method as claimed in any preceding claim, wherein: The polyol used to prepare the prepolymer has two or more OH groups.
11. A method as claimed in any preceding claim, wherein: The polyol used to prepare the prepolymer is selected from poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, and particularly preferably the alkylene group is C2-C4.
12. A method as claimed in any preceding claim, wherein: The polyol used to prepare the prepolymer is a poly(propylene oxide) polyol.
13. A method as claimed in any preceding claim, wherein: The polyol used to prepare the prepolymer is a propylene glycol-based polyether polyol with ethylene oxide end-capping, the polyether polyol having a molecular weight of about 2,000 Da and a functionality of 2.
14. A method as claimed in any preceding claim, wherein: The polyol used for preparing the prepolymer is used in an amount of 5 to 20 wt %, based on the total weight of component A, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %.
15. A method as claimed in any preceding claim, wherein: The polyol used for preparing the prepolymer is a polyether polyol based on propylene glycol, which is used in an amount of 5 to 20 wt %, based on the total weight of component A, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %.
16. A method as claimed in any preceding claim, wherein: The polyisocyanate is used in an amount in excess of the polyether polyol such that the prepolymer is terminated with isocyanate groups.
17. A method as claimed in any preceding claim, wherein: The prepolymer is terminated with isocyanate groups, wherein the NCO wt% is in the range of 5% to 30%, preferably in the range of 10% to 25%.
18. A method as claimed in any preceding claim, wherein: The aminosilane in component A preferably has the general formula I or the general formula II: Where R 1 are independently selected from C1-C6 alkyl, and R 2 Independently selected from C2-C6 alkylene.
19. As claimed in claim 18, wherein The aminosilane in component A has the general formula I, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group.
20. The method of claim 18, wherein: The aminosilane has the general formula I, R 1 is methyl, and R2 is propylene.
21. As claimed in claim 18, wherein The aminosilane in component A has the general formula II, R 1 is a C1-C2 alkyl group, and R2 is a C2-C4 alkylene group.
22. As claimed in claim 18, wherein The aminosilane has the general formula II, R 1 is methyl, and R2 is propylene.
23. A method as claimed in any preceding claim, wherein: The aminosilane in component A is bis-(trimethoxysilylpropyl)amine.
24. A method as claimed in any preceding claim, wherein: The aminosilane in component A is used in an amount of 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A.
25. A method as claimed in any preceding claim, wherein: The aminosilane in component A is bis-(trimethoxysilylpropyl)amine, which is used in an amount of 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A.
26. A method as claimed in any preceding claim, wherein: The prepolymer in component A is prepared using: 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, of polyisocyanate, based on the total weight of component A; 5-20 wt %, more preferably 8-15 wt %, particularly preferably 9-12 wt %, of polyether polyol, based on the total weight of component A; and 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of aminosilane.
27. A method as claimed in any preceding claim, wherein: The prepolymer in component A is prepared using: 35-65 wt %, more preferably 40-60 wt %, particularly preferably 45-55 wt %, based on the total weight of component A, of MDI and / or polycarbodiimide-modified MDI, or a mixture of MDI and polycarbodiimide-modified MDI; 5 to 20 wt %, more preferably 8 to 15 wt %, particularly preferably 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol, preferably based on a polyether polyol having an OH number (mg KOH / g) of 109-115; and 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of an aminosilane of the general formula II, wherein R 1 is C1-C2 alkyl, and R2 is C2-C4 alkylene, more preferably R 1 is methyl, and R2 is propylene.
28. A method as claimed in any preceding claim, wherein: The prepolymer in component A is prepared using: 45-55 wt% of a mixture of MDI and polycarbodiimide-modified MDI, based on the total weight of component A; 9 to 12 wt %, based on the total weight of component A, of a polyether polyol based on propylene glycol having an OH number (mg KOH / g) of 109-115; and 0.5-4 wt %, more preferably 1-3 wt %, particularly preferably 1.5-2.5 wt %, based on the total weight of component A, of bis-(trimethoxysilylpropyl)amine.
29. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is selected from poly(alkylene oxide) glycols, wherein the alkylene group is C2-C6, particularly preferably the alkylene group is C2-C4, and mixtures of these.
30. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is selected from poly(propylene oxide) polyols, and mixtures of these.
31. Any preceding claim, wherein: The polyether polyol used in component B is a mixture of polyols having a functionality of 2-6.
32. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is a mixture of at least one diol, at least one triol and at least one polyol having a functionality >3.
33. Any preceding claim, wherein: The polyether polyol used in component B is a mixture comprising or consisting of diols, triols and polyols having a nominal functionality of 5-6.
34. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is a mixture of poly(propylene oxide) polyols having a functionality of 2-6.
35. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is a mixture comprising or consisting of at least one poly(propylene oxide) diol, at least one poly(propylene oxide) triol and at least one poly(propylene oxide) polyol having a functionality >3.
36. A method as claimed in any preceding claim, wherein: The polyether polyol used in component B is a mixture comprising or consisting of poly(propylene oxide) diol, poly(propylene oxide) triol and poly(propylene oxide) polyol having a nominal functionality of 5-6.
37. Any preceding claim, wherein: The polyether polyol used in component B comprises, based on the total weight of the polyether polyol in component B, 46-83 wt % of polyether triol, 19-46 wt % of polyether polyol with functionality>3, and 4-15 wt % of polyether diol.
38. Any preceding claim, wherein: The polyether polyol used in component B comprises, based on the total weight of the polyether polyol in component B, 55-65 wt% of polyether triol, 25-35 wt% of polyether polyol with functionality>3, and 5-8 wt% of polyether diol.
39. Any preceding claim, wherein: The polyether polyol used in component B comprises 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with functionality>3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
40. Any preceding claim, wherein: The polyether polyol used in component B comprises 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with functionality>3, and 5-8 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B.
41. Any preceding claim, wherein: The polyether polyol used in component B is present in an amount of 35 to 70 wt %, based on the total weight of component B, more preferably 40 to 60 wt %, particularly preferably 50 to 57 wt %.
42. Any preceding claim, wherein: Component B comprises 35 to 70 wt %, more preferably 40 to 60 wt %, particularly preferably 50 to 57 wt %, of a mixture of polyether polyols, based on the total weight of component B, the mixture comprising or consisting of: (1) based on the total weight of the polyether polyol in component B, 46-83 wt% of polyether triol, 19-46 wt% of polyether polyol with a functionality > 3, and 4-15 wt% of polyether diol; or (2) based on the total weight of the polyether polyol in component B, 55-65 wt% of a polyether triol, 25-35 wt% of a polyether polyol having a functionality > 3, and 5-8 wt% of a polyether diol; or (3) 46-83 wt% of poly(propylene oxide) triol, 19-46 wt% of poly(propylene oxide) polyol with functionality>3, and 4-15 wt% of poly(propylene oxide) diol, based on the total weight of the polyether polyol in component B; or (4) Based on the total weight of the polyether polyol in component B, 55-65 wt% of poly(propylene oxide) triol, 25-35 wt% of poly(propylene oxide) polyol with a functionality > 3, and 5-8 wt% of poly(propylene oxide) diol.
43. Any preceding claim, wherein: Component B comprises diols having a molecular weight <200 Da, more preferably <150 Da.
44. Any preceding claim, wherein: Component B comprises a diol selected from propylene glycol, butylene glycol, and mixtures of these.
45. Any preceding claim, wherein: Component B comprises butanediol (eg 1,4-butanediol), which is particularly preferred.
46. Any preceding claim, wherein: Component B comprises 5 to 12 wt %, more preferably 6-10 wt %, particularly preferably 8-9 wt %, based on the total weight of component B, of diols having a molecular weight <200 Da.
47. Any preceding claim, wherein: Component B comprises 5 to 12 wt %, more preferably 6-10 wt %, particularly preferably 8-9 wt %, of butanediol (eg 1,4-butanediol), based on the total weight of component B.
48. Any preceding claim, wherein: The catalyst is selected from Lewis bases and Lewis acids.
49. Any preceding claim, wherein: The catalyst includes a catalyst selected from diazabicyclo[2.2.2]octane, tris-2,4,6-((dimethylamino)methyl)phenol, DMDEE (2,2'-dimorpholinodiethyl ether), imidazole (such as 4-methylimidazole), triethanolamine, polyethyleneimine, and mixtures thereof.
50. Any preceding claim, wherein: The catalyst includes diazabicyclo[2.2.2]octane.
51. Any preceding claim, wherein: The catalyst includes an organotin compound.
52. Any preceding claim, wherein: The catalyst comprises an organotin compound selected from dioctyl dineodecanoyl oxide tin, dibutyltin di(acetate), and di-n-octyltin bis(isooctyl thioglycolate), and mixtures thereof.
53. Any preceding claim, wherein: The catalyst includes dibutyltin di(acetate).
54. Any preceding claim, wherein: The catalyst includes diazabicyclo[2.2.2]octane and dibutyltin di(acetate).
55. Any preceding claim, wherein: The catalyst is used in an amount of 0.05-0.5 wt %, based on the total weight of component B, more preferably 0.1-0.3 wt %, particularly preferably 0.2 wt %.
56. Any preceding claim, wherein: The catalyst is a mixture of diazabicyclo[2.2.2]octane and dibutyltin diacetate, which is used in an amount of 0.05-0.5 wt %, more preferably 0.1-0.3 wt %, particularly preferably 0.2 wt %, based on the total weight of component B.
57. Any preceding claim, wherein: The concentration of the aluminum hydroxide in the binder mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) is 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture.
58. Any preceding claim, wherein: The aluminum hydroxide is present in component A at 20-35 wt %, more preferably 22-26 wt %, based on the total weight of component A.
59. Any preceding claim, wherein: The aluminum hydroxide is present in component B at 20-35 wt %, more preferably 22-26 wt %, based on the total weight of component B.
60. Any preceding claim, wherein: The aluminum hydroxide is present in both component A and component B.
61. Any preceding claim, wherein: The aluminum hydroxide is present in both component A and component B at 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components.
62. Any preceding claim, wherein: The aluminum hydroxide has a D of less than 3 microns, more preferably about 1 micron. 50 .
63. Any preceding claim, wherein: The adhesive mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) contains 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the mixture, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
64. Any preceding claim, wherein: Component A comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component A, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
65. Any preceding claim, wherein: Component B comprises 20-35 wt%, more preferably 22-26 wt%, based on the total weight of component B, of a D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
66. Any preceding claim, wherein: Both component A and component B contain 20-35 wt%, more preferably 22-26 wt%, based on the total weight of the respective components, of D having a particle size of less than 3 microns, more preferably about 1 micron. 50 of aluminum hydroxide.
67. Any preceding claim, wherein: The concentration of the melamine polyphosphate in the adhesive mixture obtained by mixing components A and B (preferably in a volume ratio of 1:1) is 7-15 wt%, more preferably 8-12 wt%, particularly preferably 9-11 wt%, based on the total weight of the mixture.
68. Any preceding claim, wherein: Melamine polyphosphate is present in component A at 7-15 wt %, more preferably 8-12 wt %, based on the total weight of component A.
69. Any preceding claim, wherein: Melamine polyphosphate is present in component B at 7-15 wt %, based on the total weight of component B, more preferably 8-12 wt %.
70. Any preceding claim, wherein: Melamine polyphosphate is present in both component A and component B.
71. Any preceding claim, wherein: Melamine polyphosphate is present in both component A and component B at 7-15 wt%, more preferably 8-12 wt%, based on the total weight of the respective components.
72. Any preceding claim, wherein: When measured according to the method given in the examples, the cured adhesive composition obtained by mixing components A and B, after being cured at 23° C., 50% relative humidity and left to stand for 7 days, has an overlap shear strength on an aluminum substrate of preferably 8 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
73. Any preceding claim, wherein: When measured according to the method given in the example, the cured adhesive composition obtained by mixing components A and B is cured at 23°C, 50% relative humidity and left to stand for 7 days, followed by 7 days of poultice treatment, and the lap shear strength on the aluminum substrate is preferably 6 MPa or greater, more preferably 9 MPa or greater, and particularly preferably 10 MPa or greater.
74. Any preceding claim, wherein: When measured according to the method given in the examples, the lap shear strength of the cured adhesive composition obtained by mixing components A and B, after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and then cured at 85°C and 85% relative humidity and left to stand for 168 hours, on an aluminum substrate is preferably 8 MPa or more, more preferably 10 MPa or more, and particularly preferably 11 MPa or more.
75. Any preceding claim, wherein: When measured according to the method given in the examples, the lap shear strength on an aluminum substrate of the cured adhesive composition obtained by mixing components A and B, after being cured at 23° C., 50% relative humidity and left to stand for 7 days, and then cured at 85° C. and 85% relative humidity and left to stand for 1,000 hours, is preferably 8 MPa or more, more preferably 10 MPa or more, and particularly preferably 11 MPa or more.
76. Any preceding claim, wherein: The cured adhesive composition obtained by mixing components A and B preferably has a UL94 rating of V0 after curing for 7 days at 23° C. and 50% relative humidity.
77. Any preceding claim, wherein: When measured according to the method given in the examples, the cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength on an aluminum substrate of 8 MPa or more, more preferably 9 MPa or more, particularly preferably 10 MPa or more, after being cured at 23°C and 50% relative humidity and left to stand for 7 days, and has a UL94 rating of V0 after being cured at 23°C and 50% relative humidity for 7 days.
78. Any preceding claim, wherein: When measured according to the method given in the examples, the cured adhesive (7 days at 23°C and 50% relative humidity) has a lap shear strength of 6 MPa or greater, more preferably 9 MPa or greater, particularly preferably 10 MPa or greater on an aluminum substrate after 7 days of poultice treatment, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
79. Any preceding claim, wherein: The cured adhesive has a lap shear strength of 8 MPa or more, more preferably 10 MPa or more, particularly preferably 11 MPa or more, on an aluminum substrate after 168 hours at 85°C and 85% relative humidity (7 days) when measured according to the method given in the examples, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
80. Any preceding claim, wherein: The cured adhesive composition obtained by mixing components A and B (at 23°C and 50% relative humidity for 7 days) has a lap shear strength of 8 MPa or more, more preferably 10 MPa or more, particularly preferably 11 MPa or more, on an aluminum substrate after 1,000 hours at 85°C and 85% relative humidity, when measured according to the method given in the examples, and has a UL94 rating of V0 after curing at 23°C and 50% relative humidity for 7 days.
Citation Information
Cited By
Polyurethane as well as preparation method and application thereof
CN119798587A